Anti-glare film and preparation method thereof

By using silicone modified polyacrylate and nanometal oxide powder and combining with the high light transmittance of polymethyl methacrylate, the performance of the anti-glare film is optimized, and the haze and hardness caused by excessive inorganic particles are solved. Reduce the problem and achieves an anti-glare film with high hardness, low haze and excellent anti-glare effect.

CN118006230BActive Publication Date: 2024-11-08深圳市精恒光电科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410113580.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-26
Publication Date
2024-11-08
Estimated Expiration
2044-01-26

AI Technical Summary

Technical Problem

When the existing anti-glare films increase inorganic particles to improve roughness and hardness, it is easy to cause a decrease in haze and gloss, affecting the use effect.

Method used

Using silicone modified polyacrylate, acrylic resin, nanometal oxide powder and curing agent, a high-hardness anti-glare film layer is formed through cross-linking reaction, and the particle size and amount of nanometal oxide powder are strictly controlled. , combined with the high light transmittance of polymethyl methacrylate, optimize the performance of the anti-glare film.

Benefits of technology

It realizes excellent anti-glare effect, high hardness, low haze, high light transmittance and good adhesion of the anti-glare film, and solves the problems of haze and hardness reduction caused by excessive inorganic particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004684272510000051
    Figure BDA0004684272510000051
  • Figure BDA0004684272510000061
    Figure BDA0004684272510000061
  • Figure BDA0004684272510000062
    Figure BDA0004684272510000062
Patent Text Reader

Abstract

The present application relates to the technical field of anti-glare films, and in particular to an anti-glare film and a preparation method thereof, comprising an anti-glare film layer and an adhesive layer, wherein the anti-glare film layer is prepared from the following raw materials in parts by weight: 40-60 parts of organosilicon-modified polyacrylate, 20-30 parts of acrylic resin, 15-20 parts of polymethyl methacrylate, 10-20 parts of nano-metal oxide powder, 1-2 parts of curing agent and 60-70 parts of diluent, wherein the acrylic resin and organosilicon-modified polyacrylate are used in combination, and a cross-linking reaction occurs after curing to form an anti-glare film layer with high hardness, thereby improving the wear resistance of the anti-glare film layer, and the addition of nano-metal oxide powder and polymethyl methacrylate improves the anti-glare effect and light transmittance of the anti-glare film, and through the combination and use of the above raw materials, the anti-glare film layer has good hardness, friction resistance, light transmittance, and low haze.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of anti-glare films, and in particular to an anti-glare film and a preparation method thereof. Background Art

[0002] With the development of electronic products such as touch-screen mobile phones, tablets and computers, people use electronic screens for longer periods of time. Electronic screens generate a lot of glare, which can cause people to have refractive errors or visual impairments. In order to prevent the harm of glare, anti-glare film is pasted on the surface of the electronic screen. Anti-glare film can reduce light reflection and scattering. When light shines on the surface of the anti-glare film, the film material will change the propagation path of the light and selectively absorb part of the light. The reflected and scattered light will be reduced, thereby reducing the intensity of the glare. Anti-glare film can effectively reduce about 55% of the glare and 65% of the reflection from the screen. Using anti-glare film can reduce the risk of eye glare discomfort, prevent visual fatigue and protect eye health.

[0003] Most of the existing anti-glare films are prepared by mixing inorganic particles with an adhesive resin, coating them on a substrate, and then forming a light diffusion layer by ultraviolet or thermal curing. Inorganic or light scattering particles are evenly dispersed in the film, and the roughness of the surface of the anti-glare film is increased by inorganic particles, so that the anti-glare film has light scattering and anti-glare effects. The higher the surface roughness of the anti-glare film, the better its anti-glare performance, and the more inorganic particles are used. However, the more inorganic particles there are, the higher the haze of the anti-glare film will be. The higher the haze, the lower the clarity and gloss, which affects the use of the anti-glare film. Therefore, in practical applications, in order to balance the roughness and haze, the amount of inorganic particles will not be added too much, usually 5-15% of the total amount, which will result in the roughness and hardness of the anti-glare film not being prominent. Therefore, it is necessary to design an anti-glare film with good roughness, good hardness and low haze. Summary of the invention

[0004] In order to solve the problem that adding too much inorganic particles will lead to increased haze of the anti-glare film, and reducing the amount of inorganic particles will lead to reduced hardness and roughness of the anti-glare film, the present application provides an anti-glare film and a preparation method thereof.

[0005] In a first aspect, the present application provides an anti-glare film, which adopts the following technical solution:

[0006] An anti-glare film, comprising an anti-glare film layer and an adhesive layer, wherein the anti-glare film layer is prepared from the following raw materials in parts by weight: 40-60 parts of organosilicon-modified polyacrylate

[0007] Acrylic resin 20-30 parts

[0008] Polymethyl methacrylate 15-20 parts

[0009] 10-20 parts of nano metal oxide powder 1-2 parts of curing agent

[0010] 60-70 parts of diluent.

[0011] By adopting the above technical solution, the prepared anti-glare film has excellent anti-glare effect, high hardness, good roughness, low haze, high light transmittance, good adhesion and flexibility. The present application uses acrylic resin and silicone modified polyacrylate together, and after curing, a cross-linking reaction occurs to form a high-hardness anti-glare film layer, thereby improving the wear resistance of the anti-glare film layer. At the same time, the network structure formed by acrylic resin and silicone modified polyacrylate can reduce the reflection and scattering of light.

[0012] The refractive effect of nano-metal oxide powder is better than that of general inorganic fillers. Adding nano-metal oxide powder and evenly distributing the metal oxide powder in the anti-glare film layer can improve the anti-glare effect of the anti-glare film. At the same time, nano-metal oxide powder has different particle sizes, which can reduce the scattering and reflection of light. Nano-metal oxide powder cooperates with acrylic resin, silicone-modified polyacrylate and common, so that the anti-glare film layer has good hardness and roughness, which can solve the problem well. The more inorganic particles, the higher the haze of the anti-glare film, and the higher the haze, the lower the clarity and gloss. At the same time, adding an appropriate amount of nano-metal oxide powder is beneficial to improve the hardness and wear resistance of the anti-glare film.

[0013] The addition of nano-metal oxide powder will reduce the transmittance of the anti-glare film layer, while the higher transmittance of polymethyl methacrylate can improve the problem of reduced transmittance caused by nano-metal oxide powder. Using it to prepare anti-glare film can further improve the transmittance of the anti-glare film.

[0014] Preferably, the average particle size of the nano metal oxide powder is 20-50 nm. By strictly controlling the particle size range of the nano metal oxide powder, the roughness of the surface of the anti-glare film can be controlled and the haze can be reduced.

[0015] The curing agent is used to promote the curing of the anti-glare film layer, which is beneficial to the formation of a film layer with a stable structure; the diluent is used to adjust the viscosity of the silicone-modified polyacrylate system, which is beneficial to roll coating and film formation.

[0016] The adhesive layer is used to bond the anti-glare film to the adhered object to ensure that the anti-glare film does not fall off.

[0017] Preferably, the organosilicon-modified polyacrylate is prepared from the following raw materials in parts by weight:

[0018] 40-70 parts of silicone monomer

[0019] Acrylic acid functional monomer 20-40 parts

[0020] Initiator 1-3 parts

[0021] Solvent 50-90 parts

[0022] 10-15 parts of triethylamine.

[0023] Preferably, the organosilicon-modified polyacrylate is prepared by the following method:

[0024] 1) mixing 1 / 3-1 / 2 of an organosilicon monomer, 1 / 4-1 / 3 of an acrylic functional monomer, 1 / 5-1 / 4 of an initiator and 1 / 2 of a solvent to obtain a mixture A;

[0025] 2) 1 / 4-1 / 3 of acrylic functional monomer, 1 / 5-1 / 4 of initiator and remaining solvent are placed in a reactor, heated to 70-80° C., stirred for 20-40 minutes, and then mixture A is added dropwise. After the addition is completed, the temperature is raised to 100-110° C. and kept warm for 1-2 hours to obtain a prepolymer; 3) The remaining silicone monomer, the remaining acrylic functional monomer and the remaining initiator are mixed, heated to 70-80° C., cooled to 40-45° C., triethylamine is added, and the pH is adjusted to 6.0-6.5 to obtain silicone-modified polyacrylate.

[0026] By adopting the above technical scheme, the prepared organosilicon-modified polyacrylate is used for preparing anti-glare film, which can further improve the hardness, wear resistance and light transmittance of the anti-glare film, and reduce the haze of the anti-glare film. By polymerizing the organosilicon monomer and the acrylic functional monomer, siloxane is introduced into the main chain, which improves the structural stability of the organosilicon-modified polyacrylate and makes it have good wear resistance and hardness. The preparation efficiency of the organosilicon-modified polyacrylate by the above steps is high, and the light transmittance and clarity are high after curing. In this application, it is necessary to introduce more organosilicon monomers. In order to make the organosilicon monomers fully react, in this application, the organosilicon monomers are reacted twice. In step 2), part of the organosilicon monomers are first introduced to form a prepolymer; and then in 3), the monomer organosilicon is introduced again by reacting the prepolymer, the remaining organosilicon monomers, the acrylic functional monomers, and the initiator, so as to introduce more siloxane.

[0027] The synthesis efficiency of organosilicon-modified polyacrylate is improved by optimizing the dosage of raw materials used in preparing organosilicon-modified polyacrylate.

[0028] Preferably, the organosilicon monomer includes at least one of vinyl trimethoxysilane, vinyl triethoxysilane, methacryloxypropyl trimethoxysilane, isocyanate propyl triethoxysilane, 3-glycidyloxypropyl trimethoxysilane or 3-mercaptopropyl trimethoxysilane.

[0029] By adopting the above technical solution, the light transmittance, wear resistance and hardness of the organosilicon-modified polyacrylate after curing are improved. The above organosilicon monomer can improve the synthesis efficiency of the organosilicon-modified polyacrylate and can introduce more siloxane.

[0030] Preferably, the acrylic functional monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-methylbutyl acrylate, isopentyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, isooctyl acrylate and isobornyl acrylate.

[0031] By adopting the above technical scheme, the wear resistance, hardness and light transmittance of the organosilicon-modified polyacrylate after curing are improved, and the film-forming property of the organosilicon-modified polyacrylate is improved, making it easier to cure to form a stable network structure.

[0032] Preferably, the acrylic resin has a viscosity of 250-3000 mPa.s at 25° C. and a molecular weight of 8000-20000.

[0033] By adopting the above technical solution, the parameters of acrylic resin are optimized, the curing of acrylic resin and silicone-modified polyacrylate is further promoted, the hardness, wear resistance and light transmittance of the anti-glare film layer are improved, and the haze of the anti-glare film is reduced.

[0034] Preferably, the nano metal oxide powder includes at least one of titanium dioxide, silicon dioxide and zirconium dioxide.

[0035] By adopting the above technical solution, the refractive effect of the anti-glare film layer is further increased, thereby improving the anti-glare effect of the anti-glare film layer. Experiments have proved that the anti-glare effect is best when the above nano metal oxide powder is used.

[0036] Preferably, the molecular weight of the polymethyl methacrylate is 5000-20000.

[0037] By adopting the above technical solution, the molecular weight of polymethyl methacrylate is optimized to further improve the light transmittance of the anti-glare film, and at the same time, the haze of the anti-glare film can be reduced.

[0038] Preferably, the anti-glare film layer has a thickness of 130-140 μm, and the adhesive layer has a thickness of 20-25 μm.

[0039] By adopting the above technical solution, the thickness of the anti-glare film layer and the adhesive layer is optimized, which is beneficial to improving the bonding stability of the anti-glare film and preventing the anti-glare film from falling off, while ensuring the light transmittance and anti-glare effect of the anti-glare film.

[0040] In a second aspect, the present application provides a method for preparing an anti-glare film, using a technical solution such as:

[0041] A method for preparing an anti-glare film comprises the following preparation steps:

[0042] S1, mixing polymethyl methacrylate and a diluent and heating until the polymethyl methacrylate is dissolved to obtain a polymethyl methacrylate solution;

[0043] S2, fully mixing the polymethyl methacrylate solution, silicone-modified polyacrylate, acrylic resin, nano-metal oxide powder and curing agent to obtain an anti-glare liquid;

[0044] S3, evenly coating the anti-glare coating liquid on the release film by roller coating or other methods, baking and drying, and curing to obtain an anti-glare film layer, coating the surface of the anti-glare film layer with optical glue, curing to form an adhesive layer, and attaching a protective film to obtain a finished product.

[0045] By adopting the above technical solution, the anti-glare film prepared has excellent anti-glare effect, high hardness, good roughness, low haze, high light transmittance, good adhesion and flexibility. By mixing and heating the polymethyl methacrylate and the diluent, it is beneficial for the polymethyl methacrylate to be fully mixed with the silicone-modified polyacrylate and the acrylic resin, which is beneficial for the subsequent curing and film formation.

[0046] The release film and protective film need to be removed during use.

[0047] In summary, this application has the following beneficial effects:

[0048] 1. The anti-glare film of the present application comprises an anti-glare layer and an adhesive layer, wherein the anti-glare layer is prepared from silicone-modified polyacrylate, polymethyl methacrylate, acrylic resin, nano-metal oxide powder, curing agent and diluent, and the silicone-modified polyacrylate and acrylic resin are cross-linked and cured to form a network structure, which can reduce the reflection and scattering of light, and at the same time, the refraction of the nano-metal oxide powder is used to further reduce the reflection and scattering of light, and adding polymethyl methacrylate with high light transmittance to prepare the anti-glare film can further improve the light transmittance of the anti-glare film.

[0049] 2. The present application prepares silicone-modified polyacrylate for use in preparing anti-glare film by mixing silicone monomer, acrylic functional monomer, initiator, solvent and triethylamine in a specific proportion and preparation method, which can further improve the hardness, abrasion resistance and light transmittance of the anti-glare film and reduce the haze of the anti-glare film. DETAILED DESCRIPTION

[0050] Example

[0051] Example 1

[0052] An anti-glare film comprises an anti-glare film layer and an adhesive layer, wherein the thickness of the anti-glare film layer is 130 μm, and the thickness of the adhesive layer is 20 μm, and is prepared by the following method:

[0053] S1, mixing 150 g of polymethyl methacrylate and 600 g of a diluent (ethyl acetate) and heating until the polymethyl methacrylate is dissolved to obtain a polymethyl methacrylate solution;

[0054] S2. Fully mix polymethyl methacrylate solution, 400 g of silicone-modified polyacrylate, 200 g of acrylic resin, 100 g of nano-metal oxide powder (silicon dioxide) and 10 g of curing agent (dodecenylsuccinic anhydride) to obtain an anti-glare liquid; S3. Evenly apply the anti-glare liquid coating liquid on the release film by roller coating or the like, bake and dry, and solidify to obtain an anti-glare film layer, apply optical glue on the surface of the anti-glare film layer, solidify to form an adhesive layer, and affix a protective film to obtain a finished product.

[0055] The molecular weight of polymethyl methacrylate is 5,000.

[0056] The viscosity of the silicone-modified polyacrylate at 25° C. is 2000 mPa.s, the molecular weight is 2500, and the hydroxyl content is 30 mgKOH / g.

[0057] The viscosity of acrylic resin at 25°C is 250mPa.s and the molecular weight is 8000.

[0058] The difference between Example 2-3 and Example 1 is that the types and amounts of raw materials used to prepare the anti-glare film layer are partially different. The specific differences are shown in Table 1:

[0059] Table 1 Types and amounts of raw materials used in preparing anti-glare film layers in Examples 1-3

[0060]

[0061]

[0062] Example 4

[0063] An anti-glare film, this embodiment is different from embodiment 1 in that the organosilicon-modified polyacrylate is prepared by the following method:

[0064] 1) 133.3 g of an organosilicon monomer (vinyl trimethoxysilane), 50 g of an acrylic functional monomer (methyl acrylate), 2 g of an initiator (ditoluoyl peroxide) and 250 g of a solvent (ethyl acetate) were mixed to obtain a mixture A;

[0065] 2) 50 g of acrylic acid functional monomer (methyl acrylate), 2 g of initiator (xylene peroxide) and 250 g of solvent (ethyl acetate) were placed in a reactor, heated to 70° C., stirred for 20 min, and then mixture A was added dropwise. After the addition was completed, the temperature was raised to 100° C. and kept warm for 1 h to obtain a prepolymer;

[0066] 3) 266.7 g of organosilicon monomer (vinyl trimethoxysilane), 100 g of acrylic functional monomer (methyl acrylate) and 6 g of initiator (xylene peroxide) were mixed, the temperature was raised to 70° C., the temperature was lowered to 40° C., 100 g of triethylamine was added, and the pH was adjusted to 6.0 to obtain organosilicon-modified polyacrylate.

[0067] The difference between Example 5-6 and Example 4 is that the raw materials, types and experimental parameters for preparing the organosilicon-modified polyacrylate are partially different. The specific differences are shown in Table 2:

[0068] Table 2 Raw materials, types and experimental parameters for preparing silicone-modified polyacrylates in Examples 4-6

[0069]

[0070]

[0071] Example 7

[0072] An anti-glare film, the difference between this embodiment and embodiment 4 is that the steps in step 2 are as follows:

[0073] Mix 400 g of silicone monomer (vinyl trimethoxysilane), 100 g of acrylic functional monomer (methyl acrylate), 4 g of initiator (xylene peroxide) and 500 g of solvent (ethyl acetate), place in a reactor, heat to 70° C., stir for 20 min, continue stirring for the same time as the time for adding mixture A in the embodiment, heat to 100° C., and keep warm for 1 h to obtain a prepolymer.

[0074] No organosilicon monomer is added in step 1), and no organosilicon sub-monomer is added in step 3), but the remaining steps are consistent with Example 4.

[0075] Example 8

[0076] An anti-glare film is disclosed. The difference between this embodiment and embodiment 1 is that the silicone monomer includes 200 g of vinyl trimethoxy silane and 200 g of 3-glycidyloxypropyl trimethoxy silane, and the types, amounts and experimental steps of other raw materials are consistent with those in embodiment 1.

[0077] Example 9

[0078] An anti-glare film is disclosed. The difference between this embodiment and embodiment 1 is that the acrylic functional monomer includes 100 g of methyl acrylate and 100 g of isooctyl acrylate, and the types, amounts and experimental steps of other raw materials are consistent with those in embodiment 1.

[0079] Example 10

[0080] An anti-glare film is disclosed. The difference between this embodiment and embodiment 1 is that zinc oxide is used to replace an equal amount of silicon dioxide, and the types, amounts and experimental steps of other raw materials are consistent with those of embodiment 1.

[0081] Comparative Example

[0082] Comparative Example 1

[0083] An anti-glare film is disclosed. The difference between this comparative example and Example 1 is that silicone-modified polyurethane is used to replace an equal amount of silicone-modified polyacrylate, and the types, amounts and experimental steps of other raw materials are consistent with those of Example 1.

[0084] The viscosity of the silicone-modified polyurethane at 25°C is 2000 mPa.s and the molecular weight is 2500.

[0085] Comparative Example 2

[0086] An anti-glare film is disclosed. The difference between this comparative example and Example 1 is that epoxy resin is used instead of an equal amount of acrylic resin, and the types, amounts and experimental steps of other raw materials are consistent with those of Example 1.

[0087] The viscosity of the epoxy resin at 25 is 250mPa.s, the molecular weight is 8000, and the epoxy value is 12eq / 100g.

[0088] Comparative Example 3

[0089] An anti-glare film is disclosed. The difference between this comparative example and Example 1 is that polystyrene is used to replace an equal amount of polymethyl methacrylate, and the types, amounts and experimental steps of other raw materials are consistent with those of Example 1.

[0090] The molecular weight of polystyrene is 5000.

[0091] Comparative Example 4

[0092] An anti-glare film is disclosed. The difference between this comparative example and Example 1 is that an equal amount of talcum powder is used to replace silicon dioxide, and the types, amounts and experimental steps of other raw materials are consistent with those of Example 1.

[0093] Performance testing

[0094] The anti-glare films prepared in Examples 1-10 and the anti-glare films prepared in Comparative Examples 1-4 were subjected to hardness test, friction resistance test, light transmittance test and haze test.

[0095] Detection method / test method

[0096] Hardness test: GB / T6739-1996 coating hardness pencil is used for determination.

[0097] Wear resistance test: 0000# steel wool, 1000g load, 1cm*1cm contact area, friction speed of 60 times / min, observe under a microscope and see if there is no damage. The wear resistance is OK, otherwise it is NG.

[0098] Light transmittance: Refer to JISK7361.

[0099] Haze: Refer to JISK7136. The experimental data is shown in Table 3:

[0100] Table 3 Experimental data of Examples 1-10 and Comparative Examples 1-3

[0101]

[0102] From Examples 1-9 and Comparative Examples 1-3 in combination with Table 3, it can be seen that the anti-glare film prepared by the present application has good hardness, abrasion resistance and light transmittance, as well as the property of low haze.

[0103] By comparing Example 1 with Comparative Example 1, the hardness in Comparative Example 1 is HB, the friction resistance test result is NG, the transmittance is 85.6%, and the haze is 8.9%, which indicates that the addition of silicone-modified polyacrylate in the present application is beneficial to improving the hardness, friction resistance and light transmittance of the anti-glare film layer, and can significantly reduce the haze of the anti-glare film layer.

[0104] Comparing Example 1 with Comparative Example 2, the hardness in Comparative Example 2 is B, the friction resistance test result is NG, the transmittance is 88.3%, and the haze is 7.6%, indicating that the addition of acrylic resin in the present application is beneficial to improving the hardness, friction resistance and light transmittance of the anti-glare film layer, and can significantly reduce the haze of the anti-glare film layer.

[0105] Comparing Example 1 with Comparative Example 3, the hardness in Comparative Example 3 is H, the friction resistance test result is NG, the transmittance is 91.2%, and the haze is 10.9%, indicating that the addition of polymethyl methacrylate in the present application is beneficial to improving the hardness, friction resistance and light transmittance of the anti-glare film layer, and can significantly reduce the haze of the anti-glare film layer.

[0106] Comparing Example 1 with Comparative Example 4, the hardness in Comparative Example 4 is H, the friction resistance test result is NG, the transmittance is 90.1%, and the haze is 5.6%, indicating that the addition of silica in the present application is beneficial to improving the hardness, friction resistance and light transmittance of the anti-glare film layer, and can significantly reduce the haze of the anti-glare film layer.

[0107] Compared with Example 1 and Example 4, and Example 4 and Example 7, the hardness and transmittance in Example 4 are improved, and the haze is significantly reduced, indicating that the hardness and transmittance of the anti-glare film can be further improved and the haze of the anti-glare film can be reduced by preparing the silicone-modified polyacrylate by the preparation method of the present application.

[0108] Compared with Example 1 and Examples 8-9, the hardness and transmittance of Examples 8-9 are improved, and the haze is reduced, which shows that the combination of different silicone monomers and acrylic functional monomers is beneficial to improving the hardness and transmittance of the anti-glare film and reducing the haze of the anti-glare film.

[0109] Compared with Example 1, the haze in Example 10 is improved, which indicates that the addition of silicon dioxide is beneficial to reducing the haze of the anti-glare film layer.

[0110] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-glare film, characterized in that: It comprises an anti-glare film layer and an adhesive layer, and the anti-glare film layer is prepared from the following raw materials in parts by weight: 40-60 parts of silicone modified polyacrylate Acrylic resin 20-30 parts Polymethyl methacrylate 15-20 parts 10-20 parts of nano metal oxide powder 1-2 parts of curing agent 60-70 parts of diluent; The nano metal oxide powder includes at least one of titanium dioxide and zirconium dioxide; The average particle size of the nano metal oxide powder is 20-50 nm; The molecular weight of the polymethyl methacrylate is 5000-20000; The organosilicon-modified polyacrylate is prepared from the following raw materials in parts by weight: 40-70 parts of silicone monomer Acrylic acid functional monomer 20-40 parts Initiator 1-3 parts Solvent 50-90 parts 10-15 parts of triethylamine; The organosilicon-modified polyacrylate is prepared by the following method: 1) Mix 1 / 3-1 / 2 of silicone monomer, 1 / 4-1 / 3 of acrylic functional monomer, 1 / 5-1 / 4 of initiator and 1 / 2 of solvent to obtain mixture A; 2) Place 1 / 4-1 / 3 of acrylic acid functional monomer, 1 / 5-1 / 4 of initiator and the remaining solvent in a reactor, heat to 70-80°C, stir for 20-40 minutes, then drop mixture A, and after the addition is complete, heat to 100-110°C and keep warm for 1-2 hours to obtain a prepolymer; 3) Mix the remaining silicone monomer, the remaining acrylic functional monomer and the remaining initiator, raise the temperature to 70-80°C, lower the temperature to 40-45°C, add triethylamine, and adjust the pH to 6.0-6.5 to obtain silicone-modified polyacrylate; The organosilicon monomer includes at least one of vinyl trimethoxysilane, vinyl triethoxysilane, methacryloxypropyl trimethoxysilane or 3-mercaptopropyl trimethoxysilane; The acrylic resin has a viscosity of 250-3000 mpa.s at 25° C. and a molecular weight of 8000-20000.

2. The anti-glare film according to claim 1, characterized in that: The acrylic functional monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-methylbutyl acrylate, isopentyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, isooctyl acrylate and isobornyl acrylate.

3. The anti-glare film according to claim 1, characterized in that: The thickness of the anti-glare film layer is 130-140 μm, and the thickness of the adhesive layer is 20-25 μm.

4. A method for preparing the anti-glare film according to any one of claims 1 to 3, characterized in that: The method comprises the following preparation steps: S1, mixing polymethyl methacrylate and a diluent and heating until the polymethyl methacrylate is dissolved to obtain a polymethyl methacrylate solution; S2, fully mixing the polymethyl methacrylate solution, silicone-modified polyacrylate, acrylic resin, nano-metal oxide powder and curing agent to obtain an anti-glare liquid; S3, evenly coating the anti-glare coating liquid on the release film by roller coating, baking and drying, and curing to obtain an anti-glare film layer, coating the surface of the anti-glare film layer with optical glue, curing to form an adhesive layer, and attaching a protective film to obtain a finished product.