Layered catalyst reactor system and method for hydroprocessing hydrocarbon feedstocks

By adopting a layered loading and self-loading catalyst layer in the hydrotreatment catalyst system, the temperature runaway problem is solved, the activity and efficiency of hydrotreatment are improved, and more efficient catalyst use and product quality are achieved.

CN118019584BActive Publication Date: 2024-12-06CHEVRON USA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280063209.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-08-13
Filing Date
2022-06-28
Publication Date
2024-12-06
Estimated Expiration
2042-06-28

AI Technical Summary

Technical Problem

The existing hydrotreating catalyst system is prone to irreversible coke inactivation due to locally uncontrollable temperature increases, which reduces the efficiency and activity of hydrotreating.

Method used

Using a layered catalyst reactor system, the risk of temperature runaway is reduced and the activity and efficiency of hydrotreatment is improved by alternately configuring the layers of supported catalysts and self-supported catalysts.

Benefits of technology

It effectively reduces the risk of temperature out of control, improves the activity and efficiency of the hydrotreatment process, and ensures the stability of the catalyst and the quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004747399010000321
    Figure BDA0004747399010000321
  • Figure BDA0004747399010000331
    Figure BDA0004747399010000331
  • Figure BDA0004747399010000332
    Figure BDA0004747399010000332
Patent Text Reader

Abstract

A layered catalyst reactor system and method for hydroprocessing hydrocarbon feedstocks. The layered catalyst system reactor comprises a vertical bed including: a demetallization catalyst layer, multiple layers of supported hydroprocessing catalyst layers, and multiple alternating layers of supported hydrocracking catalyst and self-supported hydroprocessing catalyst. The arrangement of the catalyst layers mitigates the risk of temperature runaway and improves hydroprocessing performance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims priority to U.S. patent application No. 17 / 401,757, filed on August 13, 2021, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to a layered catalyst reactor system and method for hydrocarbon reforming. Background Art

[0004] Catalytic hydroprocessing refers to a petroleum refining process in which a carbonaceous feedstock is contacted with hydrogen and a catalyst at elevated temperature and pressure for the purpose of removing undesirable impurities and / or converting the feedstock into improved products. Examples of hydroprocessing processes include hydrotreating, hydrodemetallization, hydrocracking, and hydroisomerization processes.

[0005] Hydroprocessing processes are used to remove impurities such as sulfur, nitrogen and oxygen to control final product specifications or to prepare feeds for further processing. Supported mixed metal catalysts for hydroprocessing carbonaceous feedstocks comprise a porous alumina matrix impregnated with a combination of nickel, molybdenum, tungsten and / or cobalt. Self-supported mixed metal sulfide catalysts that are not diluted by a support pack more metal sulfides into a smaller reactor volume than supported mixed metal sulfide catalysts and therefore have greater hydrogenation capacity.

[0006] However, self-supported catalysts are more susceptible to localized "runaway" temperature increases than supported catalysts. This runaway temperature increase occurs when the hydrogenation catalyst generates more heat than its environment can absorb, becoming hotter than the bed or reactor temperature. Eventually the temperature increase accelerates hydrogen consumption, which further increases the catalyst temperature until the hydrogenation (hydrogen consumption) rate exceeds the hydrogen supply rate. At this stage the catalyst begins to dehydrogenate the feed, generating coke and hydrogen. This process results in irreversible coke deactivation.

[0007] Supported hydroprocessing catalysts generally comprise one or more metals deposited on a support or carrier composed of an amorphous oxide and / or a crystalline microporous material (e.g., a zeolite). A top layer of a supported hydroprocessing catalyst of appropriate size may be used to protect a bottom layer of the self-supported catalyst from excessive hydrogenation activity.

[0008] In view of the foregoing, there is a continuing need to provide improved hydroprocessing catalyst systems that minimize the risk of uncontrolled temperature increases while increasing the activity and efficiency of the hydroprocessing process. Summary of the invention

[0009] This Summary is provided to introduce various concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify required or essential features of the claimed subject matter, nor is this Summary intended to limit the scope of the claimed subject matter.

[0010] Aspects of the present invention are directed to layered catalyst reactor systems and methods for hydroprocessing hydrocarbon feedstocks.

[0011] In one aspect, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0012] (i) a layer comprising one or more demetallization catalysts which is from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0013] (ii) a layer of one or more supported hydroprocessing catalysts which is from about 17 to about 27% of the total volume of the catalyst in the vertical bed;

[0014] (iii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 15% of the total volume of the catalyst in the vertical bed;

[0015] (iv) one or more layers of self-supported hydroprocessing catalysts, which are from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0016] (v) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 15% of the total volume of the catalyst in the vertical bed;

[0017] (vi) one or more layers of self-supported hydroprocessing catalysts, which are from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0018] (vii) a layer of one or more supported hydroprocessing catalysts which is from about 2 to about 9% of the total volume of the catalyst in the vertical bed.

[0019] In another aspect, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0020] (i) a layer comprising one or more demetallization catalysts which is from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0021] (ii) a layer of one or more supported hydroprocessing catalysts which is from about 17 to about 27% of the total volume of the catalyst in the vertical bed;

[0022] (iii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0023] (iv) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0024] (v) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0025] (vi) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0026] (vii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0027] (vii) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0028] (viii) a layer of one or more supported hydroprocessing catalysts which is from about 2 to about 9% of the total volume of the catalyst in the vertical bed.

[0029] In another aspect, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0030] (i) a layer comprising one or more demetallization catalysts;

[0031] (ii) a layer of one or more supported hydroprocessing catalysts;

[0032] (iii) a layer of one or more supported hydrocracking catalysts;

[0033] (iv) a layer of one or more self-supported hydroprocessing catalysts;

[0034] (v) a layer of one or more supported hydrocracking catalysts;

[0035] (vi) a layer of one or more self-supported hydroprocessing catalysts;

[0036] (vii) a layer of one or more supported hydroprocessing catalysts;

[0037] wherein the total volume of the two layers comprising one or more self-supported hydroprocessing catalysts is from about 10 to about 50% of the total volume of the catalyst in the vertical bed; and

[0038] The total volume of the two layers containing the one or more supported hydrocracking catalysts is from about 10 to about 30% of the total volume of the catalyst in the vertical bed.

[0039] In another aspect, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0040] (i) a layer comprising one or more demetallization catalysts;

[0041] (ii) a layer of one or more supported hydroprocessing catalysts;

[0042] (iii) a layer of one or more supported hydrocracking catalysts;

[0043] (iv) a layer of one or more self-supported hydroprocessing catalysts;

[0044] (v) a layer of one or more supported hydrocracking catalysts;

[0045] (vi) a layer of one or more self-supported hydroprocessing catalysts;

[0046] (vii) a layer of one or more supported hydrocracking catalysts;

[0047] (viii) a layer of one or more self-supported hydroprocessing catalysts;

[0048] (ix) a layer of one or more supported hydroprocessing catalysts;

[0049] wherein the total volume of the three layers comprising one or more self-supported hydroprocessing catalysts is from about 9 to about 45% of the total volume of the catalyst in the vertical bed; and

[0050] The total volume of the three layers containing the one or more supported hydrocracking catalysts is from about 15 to about 30% of the total volume of the catalyst in the vertical bed.

[0051] In another aspect, the present invention relates to a method for hydroprocessing a hydrocarbon feedstock, which comprises: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen and olefins with the layered catalyst reactor system described herein in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically through the layers of the layered catalyst reactor system in sequence from top to bottom; and (iii) recovering the hydrocarbon product from the bottom of the layered catalyst reactor system.

[0052] This summary of the invention and the following detailed description provide examples and only explain the present invention. Therefore, the foregoing summary of the invention and the following detailed description should not be considered as restrictive. In addition to those features set forth herein, additional features or their variations may be provided, such as those various feature combinations and sub-combinations described in the detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (no hydrocracking or self-supported hydrotreating catalyst layer; BSU 607-56).

[0054] Figure 2 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (one hydrocracking catalyst layer and one self-supported hydrotreating catalyst layer; BSU607-57).

[0055] Figure 3 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (one hydrocracking catalyst layer and one self-supported hydrotreating catalyst layer; BSU911-160).

[0056] Figure 4 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (one hydrocracking catalyst layer and one self-supported hydrotreating catalyst layer; BSU607-59).

[0057] Figure 5 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (no hydrocracking or self-supported hydrotreating catalyst layer; BSU 612-37).

[0058] Figure 6 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (no hydrocracking or self-supported hydrotreating catalyst layer; BSU 612-38).

[0059] Figure 7 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (one hydrocracking catalyst layer and one self-supported hydrotreating catalyst layer; BSU607-60).

[0060] Figure 8 Graphically depicts normalized temperature for a hydroprocessing process utilizing an exemplary layered catalyst reactor system (two hydrocracking catalyst layers and two self-supported hydrotreating catalyst layers; BSU612-40).

[0061] Fig. 9 Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (no hydrocracking or self-supported hydrotreating catalyst layer; BSU612-39).

[0062] Fig.10Graphically depicts normalized temperature for a hydroprocessing process utilizing a comparative layered catalyst reactor system (one hydrocracking catalyst layer and one self-supported hydrotreating catalyst layer; BSU607-61).

[0063] Fig.11 Graphically depicts normalized temperature for a hydroprocessing process utilizing an exemplary layered catalyst reactor system (two hydrocracking catalyst layers and two self-supported hydrotreating catalyst layers; BSU612-41).

[0064] Fig.12 Graphically depicts normalized temperature for a hydroprocessing process utilizing an exemplary layered catalyst reactor system (two hydrocracking catalyst layers and two self-supported hydrotreating catalyst layers; BSU911-61).

[0065] Fig.13 Graphically depicts diesel yield versus hydrocracking conversion for different feeds.

[0066] definition

[0067] In order to more clearly define the terms used herein, the following definitions are provided. Unless otherwise indicated, the following definitions may apply to the present invention. If a term is used in the present invention but is not clearly defined herein, the definition from the IUPAC Chemical Glossary may apply, as long as the definition does not conflict with any other disclosure or definition of application herein or does not cause any claim to apply the definition to be unclear or unable to be realized. If any definition or usage provided by any document incorporated herein by reference conflicts with the definition or usage provided herein, the definition or usage provided herein shall prevail.

[0068] Unless otherwise specified, although compositions and methods are described using the term "comprising" a plurality of components or steps, the compositions and methods may also "consist essentially of" or "consist of" the plurality of components or steps.

[0069] The terms "a", "an" and "the" are intended to include plural alternatives, such as at least one. Unless otherwise specified, the terms "including", "with" and "having" used herein are defined as inclusive (i.e., open language).

[0070] Various numerical ranges are disclosed herein. Unless otherwise specified, when the applicant discloses or claims any type of range, the applicant's intention is to disclose or claim individually every possible value that the range can reasonably cover, including the endpoints of the range and any subranges and combinations of subranges contained therein. For example, unless excluded by additional conditions, all numerical endpoints of the ranges disclosed herein are approximate.

[0071] In this article, a value or range may be expressed as "about", from "about" a specific value and / or to "about" another specific value. When such values ​​or ranges are expressed, other disclosed embodiments include the specific value, from a specific value and / or to other specific values. Similarly, when a value is expressed as an approximation by using the antecedent "about", it will be understood that a specific value forms another embodiment. It will be further understood that multiple values ​​are disclosed, and each value is also disclosed as "about" this specific value and the value itself in this article. In another aspect, the use of the term "about" means ± 20% of the claimed value, ± 15% of the claimed value, ± 10% of the claimed value, ± 5% of the claimed value, ± 3% of the claimed value, or ± 1% of the claimed value.

[0072] "Periodic Table" refers to the version of the IUPAC Periodic Table of the Elements dated June 22, 2007, and the numbering scheme for the Periodic Table Groups is as described in Chemical and Engineering News, 63(5), 27 (1985).

[0073] "Hydrocarbon-containing" and "hydrocarbon" refer to compounds containing only carbon and hydrogen atoms. Other designations may be used to indicate the presence of specific groups, if any, in the hydrocarbon (eg, a halogenated hydrocarbon indicates the presence of one or more halogen atoms replacing an equal number of hydrogen atoms in the hydrocarbon).

[0074] "Hydroprocessing" or "hydroconversion" refers to a process in which a carbonaceous feedstock is contacted with hydrogen and a catalyst at elevated temperature and pressure for the purpose of removing undesirable impurities and / or converting the feedstock to a desired product. Such processes include, but are not limited to, methanation, water gas shift reaction, hydrogenation, hydrotreating, hydrodesulfurization, hydrodenitrogenation, hydrodemetallization, hydrodearomatization, hydroisomerization, hydrodewaxing, and hydrocracking (including selective hydrocracking). Depending on the type of hydroprocessing and the reaction conditions, the products of the hydroprocessing may exhibit improved physical properties, such as improved viscosity, viscosity index, saturate content, low temperature properties, volatility, and depolarization.

[0075] "Hydroprocessing" refers to a hydrogenation process used to remove pollutants such as nitrogen, sulfur, oxygen, and metals from liquid petroleum fractions. In certain embodiments, the hydroprocessing process removes at least about 90% of the pollutants containing nitrogen, sulfur, oxygen, and / or metals. In certain embodiments, the hydroprocessing process converts olefins and aromatics into saturated compounds.

[0076] "Hydrocracking" refers to a process of hydrogenation and dehydrogenation accompanied by cracking / splitting of hydrocarbons (eg, converting heavier hydrocarbons to lighter hydrocarbons).

[0077] With respect to catalysts (e.g., active phase materials), the term "supported" refers to a catalyst attached to a conventional material, usually a solid having a high surface area. The support material may be inert or participate in the catalytic reaction. The support material may be porous or non-porous. Typical catalyst supports include various carbons, alumina, silica, and silica-alumina (e.g., amorphous aluminosilicates), zeolites, alumina-boria, silica-alumina-magnesia, silica-alumina-titania, and materials obtained by adding other zeolites and other composite oxides thereto.

[0078] With respect to a catalyst, the term "self-supported" refers to an unsupported catalyst or a catalyst that is not attached to another material.

[0079] The terms "catalyst particle," "catalyst composition," "catalyst mixture," "catalyst system," and the like encompass the initial starting components of the composition as well as any products that may be derived from contacting those initial starting components, and this includes both heterogeneous catalyst systems and homogeneous catalyst systems or combinations.

[0080] If, for any reason (e.g., to account for a reference that the applicant may not have known when the application was filed), the applicant chooses to claim less than the entire disclosure of the invention, the applicant reserves the right to exclude or qualify as a condition any individual member of any such group of values ​​or ranges (including any subranges or combinations of subranges within a group that may be claimed as a range or in any similar manner). In addition, the applicant reserves the right to exclude or qualify as a condition any member of the claimed group.

[0081] Although any methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, the typical methods and materials are described herein.

[0082] For the purpose of describing and disclosing the constructions and methodology described in publications, such as those that can be used in conjunction with the presently described invention, all publications and patents mentioned herein are incorporated herein by reference. The publications discussed in various places of the text are provided only with respect to their disclosures prior to the filing date of the present application. Nothing herein is to be construed as an admission that the inventor has no right to disclose this invention in advance due to prior inventions. DETAILED DESCRIPTION

[0083] It is to be understood that the invention is not limited in its application to the details of construction and the arrangement of components set forth in the following description or illustrated in the drawings.

[0084] The present invention generally relates to a layered catalyst reactor system and method for hydroconversion of hydrocarbon feedstocks. The layered catalyst reactor system disclosed herein comprises a configuration of individual layers of alternating supported catalysts and self-supported catalysts, which improves the activity and effectiveness of hydroprocessing without increasing the volume of the catalyst. Specifically, the layered catalyst reactor system and method achieve non-monotonic hydrogenation activity by layering supported hydroprocessing and hydrocracking catalysts between layers of highly active self-supported hydroprocessing catalyst layers. In certain embodiments, the self-supported hydroprocessing catalyst is a mixed metal sulfide catalyst. The configuration of the catalyst layers in the reactor disclosed herein can be used to mitigate risk.

[0085] Given the same total volume of supported catalyst and self-supported catalyst, an exemplary layered catalyst reactor system in which two or more self-supported (or unsupported) hydroprocessing catalyst layers are sandwiched between supported catalyst layers is superior to a comparable system in which a supported catalyst layer is on top of a single self-supported catalyst layer.

[0086] The layered catalyst reactor system can be used for the hydroconversion of hydrocarbon feedstock or the method for upgrading petroleum feedstock. The method disclosed herein can be used to react hydrocarbon feedstock in the presence of hydrogen and layered catalyst reactor system under elevated temperature and pressure conditions to convert the feedstock into a lower molecular weight product with reduced pollutant content. Hydroconversion methods are those methods for hydrotreating or hydrocracking hydrocarbon feedstock, and may include, for example, hydrogenation, desulfurization, denitrogenation and metal removal. In one embodiment, the hydroconversion method includes hydrocracking and / or hydrotreating of hydrocarbon feedstock.

[0087] Layered Catalyst Reactor System

[0088] In one aspect, the present invention relates to a layered catalyst reactor system for hydroprocessing hydrocarbon feedstocks containing contaminants including metals, sulfur, nitrogen and olefins. The layered catalyst reactor system can be used to remove impurities such as metals, sulfur and nitrogen, and saturate olefins and aromatic compounds.

[0089] According to an embodiment, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0090] (i) a layer comprising one or more demetallization catalysts which is from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0091] (ii) a layer of one or more supported hydroprocessing catalysts which is from about 17 to about 27% of the total volume of the catalyst in the vertical bed;

[0092] (iii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 15% of the total volume of the catalyst in the vertical bed;

[0093] (iv) one or more layers of self-supported hydroprocessing catalysts, which are from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0094] (v) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 15% of the total volume of the catalyst in the vertical bed;

[0095] (vi) one or more layers of self-supported hydroprocessing catalysts, which are from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0096] (vii) a layer of one or more supported hydroprocessing catalysts which is from about 2 to about 9% of the total volume of the catalyst in the vertical bed.

[0097] As referred to herein, "the total volume of catalyst in a vertical bed" means the total volume of materials forming the self-supported catalyst and the layers of supported catalyst in the vertical bed.

[0098] In certain embodiments, the one or more layers of one or more self-supported hydroprocessing catalysts are about 9 to about 19%, or about 15 to about 25% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (iv) is about 9 to about 19% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (vi) is about 15 to about 25% of the total volume of the catalyst in the vertical bed.

[0099] In certain embodiments, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0100] (i) a layer comprising one or more demetallization catalysts which is from about 5 to about 25% of the total volume of the catalyst in the vertical bed;

[0101] (ii) a layer of one or more supported hydroprocessing catalysts which is from about 17 to about 27% of the total volume of the catalyst in the vertical bed;

[0102] (iii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0103] (iv) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0104] (v) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0105] (vi) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0106] (vii) a layer of one or more supported hydrocracking catalysts which is from about 5 to about 10% of the total volume of the catalyst in the vertical bed;

[0107] (vii) one or more layers of self-supported hydroprocessing catalysts, which are from about 3 to about 15% of the total volume of the catalyst in the vertical bed;

[0108] (viii) a layer of one or more supported hydroprocessing catalysts which is from about 2 to about 9% of the total volume of the catalyst in the vertical bed.

[0109] In certain embodiments, one or more layers of one or more self-supported hydroprocessing catalysts are about 4 to about 10% or about 10 to about 15% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (iv) is about 4 to about 10% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (vi) is about 10 to about 15% of the total volume of the catalyst in the vertical bed. In certain embodiments, layer (viii) is about 10 to about 15% of the total volume of the catalyst in the vertical bed.

[0110] In certain embodiments, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0111] (i) a layer comprising one or more demetallization catalysts;

[0112] (ii) a layer of one or more supported hydroprocessing catalysts;

[0113] (iii) a layer of one or more supported hydrocracking catalysts;

[0114] (iv) a layer of one or more self-supported hydroprocessing catalysts;

[0115] (v) a layer of one or more supported hydrocracking catalysts;

[0116] (vi) a layer of one or more self-supported hydroprocessing catalysts;

[0117] (vii) a layer of one or more supported hydroprocessing catalysts;

[0118] wherein the total volume of the two layers comprising one or more self-supported hydroprocessing catalysts is from about 10 to about 50% of the total volume of the catalyst in the vertical bed; and

[0119] The total volume of the two layers containing the one or more supported hydrocracking catalysts is from about 10 to about 30% of the total volume of the catalyst in the vertical bed.

[0120] In certain embodiments, the layered catalyst reactor system comprises a vertical bed or stack of catalyst layers arranged from top to bottom in the following order:

[0121] (i) a layer comprising one or more demetallization catalysts;

[0122] (ii) a layer of one or more supported hydroprocessing catalysts;

[0123] (iii) a layer of one or more supported hydrocracking catalysts;

[0124] (iv) a layer of one or more self-supported hydroprocessing catalysts;

[0125] (v) a layer of one or more supported hydrocracking catalysts;

[0126] (vi) a layer of one or more self-supported hydroprocessing catalysts;

[0127] (vii) a layer of one or more supported hydrocracking catalysts;

[0128] (viii) a layer of one or more self-supported hydroprocessing catalysts;

[0129] (ix) a layer of one or more supported hydroprocessing catalysts;

[0130] wherein the total volume of the three layers comprising one or more self-supported hydroprocessing catalysts is from about 9 to about 45% of the total volume of the catalyst in the vertical bed; and

[0131] The total volume of the three layers containing the one or more supported hydrocracking catalysts is from about 15 to about 30% of the total volume of the catalyst in the vertical bed.

[0132] In certain embodiments, the total volume of the layer comprising one or more demetallization catalysts is about 5 to about 25% of the total volume of catalyst in the vertical bed.In certain embodiments, the top layer comprises or consists of one or more demetallization catalysts.

[0133] In certain embodiments, the total volume of the layer comprising one or more supported hydroprocessing catalysts is about 19 to about 36% of the total volume of the catalyst in the vertical bed. In certain embodiments, the bottom layer comprises or consists of one or more supported hydroprocessing catalysts. In certain embodiments, the layer below the top layer and in contact therewith comprises or consists of one or more supported hydroprocessing catalysts.

[0134] In certain embodiments, the total volume of catalyst in the vertical bed is from about 50,000 to about 300,000 ft 3 In certain embodiments, the vertical bed has a width of about 50,000 to about 300,000 ft 3 volume.

[0135] An exemplary layered catalyst reactor system comprises multiple zones. The first zone at the top of the vertical bed is a demetallization zone, which is present in a layer comprising one or more demetallization catalysts. The demetallization zone is generally involved in removing contaminant metals from hydrocarbon feedstocks.

[0136] The second zone below the first zone is a hydroprocessing zone, which exists in a layer containing one or more supported hydroprocessing catalysts. This hydroprocessing zone is designed to selectively minimize inhibitors such as organic N, organic S, and aromatics by hydrogenation or saturation. This zone helps protect subsequent hydrocracking and hydroprocessing (e.g., hydroprocessing using self-supported catalysts) zones that may be sensitive to inhibitors.

[0137] The third, fourth, fifth and sixth zones are alternating layers of hydrocracking zones followed by hydrotreating zones, wherein hydrotreating occurs in a layer comprising one or more self-supported hydrotreating catalysts. In certain embodiments, one or more self-supported hydrotreating catalysts are mixed metal sulfide (MMS) catalysts. The MMS catalyst can be any mixed metal sulfide catalyst that is self-supported or unsupported. These catalysts have a high level of activity. In one embodiment, the MMS catalyst is a self-supported multi-metal catalyst prepared from a precursor in the form of an oxide or hydroxide. In a preferred embodiment, the precursor is in the form of a hydroxide.

[0138] The third and fifth zones, respectively below the second and fourth zones, are hydrocracking zones. Each hydrocracking zone involves hydrocracking a feed to reduce the boiling point of the feed.

[0139] The fourth and sixth zones, respectively below the third and fifth zones, are hydroprocessing zones, wherein hydroprocessing is performed by one or more self-supported hydroprocessing catalysts.

[0140] In certain embodiments, the layered catalyst reactor system comprises additional hydrocracking zones followed by additional self-supported catalyst hydrotreating zones (sixth and seventh zones).

[0141] The final zone (seventh or ninth zone) is a post-processing zone or additional hydroprocessing zone, wherein hydroprocessing occurs in a layer comprising one or more self-supported hydroprocessing catalysts.

[0142] Typically, hydrocarbon feedstock is introduced into the first zone (i.e., top layer) of the layered catalyst reactor system to produce treated effluent. Hydrogen is also introduced into the layered catalyst reactor system to promote hydrogenation reactions. The treated effluent from each layer moves to the next layer of the layered catalyst reactor system in a downward path. In this way, the initial hydrocarbon feedstock and the resulting treated effluent from each layer pass through the layered catalyst reactor system.

[0143] In certain embodiments, the layered catalyst reactor system operates at a temperature of about 715 to about 760°F, or about 700 to about 775°F.

[0144] Weight hourly space velocity (WHSV) is defined as the weight of feed flowing through per unit weight of catalyst per hour of reactor operating conditions. In certain embodiments, WHSV is from about 0.41 to about 1.1 or from about 0.4 to about 1.1 h -1 .

[0145] The liquid hourly space velocity (LHSV) is the ratio of the volume flow rate of liquid to the volume of catalyst per hour. In certain embodiments, the LHSV is from about 0.39 to about 0.81 h -1 or about 0.3 to about 0.9h -1 .

[0146] In certain embodiments, the total pressure in the layered catalyst reactor system during operation is from about 2318 to about 2350 psig, or from about 2310 to about 2360 psig.

[0147] In certain embodiments, the inlet hydrogen pressure in the layered catalyst reactor system during operation is from about 2244 to about 2310 psia, or from about 2240 to about 2320 psia.

[0148] In certain embodiments, the gas rate in the layered catalyst reactor system during operation is from about 7512 to about 8040 scfb, or from about 7500 to about 8100 scfb.

[0149] In certain embodiments, the normalized temperature of the layered catalyst reactor system during the hydroprocessing reaction is maintained below about 770°F, or below about 765°F.

[0150] Demetallization catalyst

[0151] Metal contaminants such as vanadium contaminants and nickel contaminants are removed from hydrocarbon feedstocks by contact with one or more demetallization catalysts. Typically, the demetallization catalyst according to the embodiment may be a conventional demetallization catalyst known in the art. Examples of demetallization catalysts (i.e., hydrodemetallization catalysts) include, but are not limited to, those prepared from natural aluminum silicates or synthetic alumina rich in oxides of molybdenum, cobalt, and nickel, such as nickel oxide-molybdenum oxide, cobalt oxide, molybdenum oxide, nickel oxide-tungsten oxide, all on alumina; and bauxite promoted with iron, cobalt, molybdenum, nickel, zinc, and manganese.

[0152] In certain embodiments, the demetallization catalyst is a catalyst comprising, for example, ICR 132 (available from Advanced Refining Technologies LLC).

[0153] In certain embodiments, the supported hydroprocessing catalyst layer comprises or consists of one type of supported hydroprocessing catalyst. In certain embodiments, the supported hydroprocessing catalyst layer comprises or consists of two types of supported hydroprocessing catalysts.

[0154] Supported hydroprocessing catalyst

[0155] Typically, the hydroprocessing catalyst according to the load of the embodiment may be a conventional hydroprocessing (e.g., hydrodesulfurization) catalyst known in the art. Examples of supported hydroprocessing catalysts include, but are not limited to, catalysts comprising at least one VIII group metal such as iron, cobalt or nickel and at least one VIB group metal such as molybdenum or tungsten on a relatively high surface area support material (e.g., alumina). Other suitable catalyst supports include zeolites, amorphous silica-alumina and titania-alumina. In certain embodiments, the supported hydroprocessing catalyst comprises precious metals such as Pd and Pt. More than one type of hydroprocessing catalyst may be used in the same or different beds of a layered catalyst reactor system. In certain embodiments, the VIII group metal is typically present in an amount of about 2 to about 20 weight %, or about 4 to about 12 weight %. The VIB group metal is typically present in an amount of about 5 to about 50 weight %, about 10 to about 40 weight %, or about 20 to about 30 weight %. All metal weight percentages are based on the carrier (based on the percentage of the carrier weight).

[0156] In certain embodiments, the supported hydroprocessing catalyst comprises one or more Group VIII metals selected from iron, cobalt or nickel. In certain embodiments, the supported hydroprocessing catalyst comprises one or more Group VIII metals selected from cobalt and nickel. In certain embodiments, the supported hydroprocessing catalyst comprises cobalt.

[0157] In certain embodiments, the supported hydroprocessing catalyst comprises a support material selected from the group consisting of alumina, zeolites, amorphous silica-alumina, and titania-alumina.

[0158] In certain embodiments, the supported hydroprocessing catalyst is a catalyst comprising nickel and molybdenum. In certain embodiments, the supported hydroprocessing catalyst is a catalyst comprising nickel oxide and molybdenum trioxide, such as ICR 513 (available from Advanced Refining Technologies LLC).

[0159] In certain embodiments, the supported hydroprocessing catalyst layer comprises or consists of one type of supported hydroprocessing catalyst. In certain embodiments, the supported hydroprocessing catalyst layer comprises or consists of two types of supported hydroprocessing catalysts.

[0160] Hydrocracking catalyst

[0161] Hydrocracking catalysts suitable for use in the systems and methods described herein include, but are not limited to, catalysts with cracking activity, such as catalysts containing crystalline aluminosilicates. Typically, the hydrocracking catalyst according to the embodiment may be a conventional hydrocracking catalyst known in the art. Examples of hydrocracking catalysts include, but are not limited to, catalysts comprising nickel, nickel-cobalt-molybdenum, cobalt-molybdenum and nickel-tungsten and / or nickel-molybdenum, wherein the latter two are preferred. Non-limiting examples of noble metal catalysts include those based on platinum and / or palladium. Porous support materials that can be used for both noble metal catalysts and non-noble metal catalysts include refractory oxide materials such as alumina, silica, alumina-silica, diatomaceous earth (kieselguhr), diatomaceous earth (diatomaceous earth), magnesium oxide or zirconium oxide, wherein alumina, silica, alumina-silica are preferred and most commonly used. Zeolite carriers can also be used, especially large-pore faujasite zeolites such as ultra-stable Y (USY).

[0162] Many hydrocracking catalysts are available from different commercial suppliers and can be used depending on the feedstock and product requirements; their functionality can be determined empirically. Any catalyst having the desired hydroconversion functionality can be used under the selected operating conditions, including conventional hydrocracking catalysts.

[0163] In certain embodiments, the hydrocracking catalyst is not the same as the catalyst used in the demetallization catalyst layer, the supported hydrotreating catalyst layer, or the unsupported hydrotreating catalyst layer.

[0164] In certain embodiments, the hydrocracking catalyst comprises nickel, cobalt, molybdenum and / or tungsten. In certain embodiments, the hydrocracking catalyst comprises nickel. In certain embodiments, the hydrocracking catalyst comprises nickel-cobalt-molybdenum. In certain embodiments, the hydrocracking catalyst comprises cobalt-molybdenum. In certain embodiments, the hydrocracking catalyst comprises nickel-tungsten. In certain embodiments, the hydrocracking catalyst comprises nickel-molybdenum.

[0165] In certain embodiments, the hydrocracking catalyst comprises a support material selected from refractory oxide materials such as alumina, silica, alumina-silica, kieselguhr, diatomaceous earth, magnesia or zirconia, wherein alumina, silica or alumina-silica are preferred, and zeolite supports, for example large pore faujasite such as USY.

[0166] In certain embodiments, the hydrocracking catalyst is a catalyst comprising nickel and molybdenum or nickel and tungsten, such as ICR250 (available from Advanced Refining Technologies LLC).

[0167] In certain embodiments, the hydrocracking catalyst is a supported hydrocracking catalyst. In certain embodiments, the hydrocracking catalyst layer comprises or consists of one type of hydrocracking catalyst. In certain embodiments, the hydrocracking catalyst layer comprises or consists of two types of hydrocracking catalysts.

[0168] Self-supported hydroprocessing catalyst

[0169] In certain embodiments, a self-supported hydroprocessing catalyst is an unsupported (ie, not supported on or attached to another material) hydroprocessing catalyst. Typically, a self-supported hydroprocessing catalyst has a higher activity level (by volume) than a supported hydroprocessing catalyst.

[0170] Examples of self-supported (or unsupported) hydroprocessing catalysts include, but are not limited to, unsupported multi-metallic catalysts prepared by sulfiding a catalyst precursor having the formula:

[0171] A v [(M P )OH) x (L) n y ] z (M VIB O4), where:

[0172] A is a monovalent cationic species,

[0173] M P is a promoter metal having an oxidation state of +2 or +4 selected from one or more of Group IIA, Group IIB, Group IVA and Group VIII metals (especially Group VIII metals such as Ni),

[0174] L is an organic oxygen-containing ligand (e.g., maleate), and

[0175] M VIB is a VIB Group metal (for example, one or more of Mo and W).

[0176] An important aspect of the catalyst precursor (before sulfiding) is that it is in the hydroxide form.

[0177] In one embodiment, L is selected from the group consisting of: carboxylates, carboxylic acids, aldehydes, ketones, enolate forms of aldehydes, enolate forms of ketones, and hemiacetals, and combinations thereof.

[0178] In one embodiment, A is selected from a monovalent cation such as NH4 + , other quaternary ammonium ions, organic phosphorus cations, alkali metal cations, and combinations thereof.

[0179] In one embodiment using both molybdenum and tungsten as the Group VIB metal, the molybdenum to tungsten atomic ratio (Mo:W) is about 10:1 to 1:10. In another embodiment, the ratio of Mo:W is about 1:1 to 1:5. In an embodiment using molybdenum and tungsten as the Group VIB metal, the electrically neutral catalyst precursor has the formula A v [(M P )(OH) x (L) n y ] z (Mo t W t′ In yet another embodiment using molybdenum and tungsten as the Group VIB metals, some or all of the tungsten may be replaced with chromium, wherein the ratio of (Cr+W):Mo is from about 10:1 to 1:10. In another embodiment, the ratio of (Cr+W):Mo is from about 1:1 to 1:5. In the embodiment where molybdenum, tungsten and chromium are Group VIB metals, the electrically neutral catalyst precursor has the formula A v [(M P )(OH) x (L) n y ] z (Mo t W t′ Crt″ O4).

[0180] In one embodiment, the promoter metal M P is at least one Group VIII metal, wherein M P has an oxidation state of +2, and the catalyst precursor has the formula A v [(M P )(OH) x (L) n y ] z (M VIB O4), where (v-2+2z-x*z+n*y*z)=0.

[0181] In one embodiment, the promoter metal M P is a mixture of two Group VIII metals such as Ni and Co. In yet another embodiment, M P A combination of three metals such as Ni, Co and Fe.

[0182] In M P In one embodiment of a mixture of two Group IIB metals such as Zn and Cd, the electrically neutral catalyst precursor has the formula A v [(Zn a Cd a′ )(OH) x (L) y ] z (M VIB O4). P In another embodiment of a combination of three metals such as Zn, Cd and Hg, the electrically neutral catalyst precursor has the formula A v [(Zn a Cd a′ Hg a″ )(OH) x (L) n y ] z (M VIB O4).

[0183] In M P In one embodiment of a mixture of two Group IVA metals such as Ge and Sn, the electrically neutral catalyst precursor has the formula A v [(Ge b ,Sn b′ )(OH) x (L) n y ] z (M VIB O4). PIn another embodiment of a combination of three Group IVA metals such as Ge, Sn and Pb, the electrically neutral catalyst precursor has the formula A v [(Ge b Sn b′ Pba b″ )(OH) x (L) n y ] z (M VIB O4).

[0184] Promoter Metal Component M P In one embodiment, the promoter metal (M P ) compound is in a liquid state, wherein the entire amount of the Promoter metal compound is dissolved in the liquid to form a homogeneous solution. In another embodiment, the source of Promoter metal is partially in a solid state and partially dissolved in the liquid. In a third embodiment, it is completely in a solid state.

[0185] Promoter Metal Compound M P It can be a metal salt or a mixture of metal salts selected from the group consisting of nitrates, hydrated nitrates, chlorides, hydrated chlorides, sulfates, hydrated sulfates, carbonates, formates, acetates, oxalates, citrates, maleates, fumarates, phosphates, hypophosphites, and mixtures thereof.

[0186] In one embodiment, the promoter metal M P A nickel compound that is at least partially solid, for example a water-insoluble nickel compound, such as nickel carbonate, nickel hydroxide, nickel phosphate, nickel phosphite, nickel formate, nickel fumarate, nickel sulfide, nickel molybdate, nickel tungstate, nickel oxide, a nickel alloy such as nickel-molybdenum alloy, Raney nickel, or a mixture thereof.

[0187] In one embodiment, the promoter metal M P is selected from Group IIB metals and Group VIA metals, such as zinc, cadmium, mercury, germanium, tin or lead and combinations thereof in elemental, compound or ionic form. P Also included are at least one of Ni, Co, Fe and combinations thereof in the form of elements, compounds or ions thereof.

[0188] In one embodiment, the promoter metal compound is a zinc compound that is at least partially solid, for example a zinc compound that is poorly soluble in water, such as: zinc carbonate, zinc hydroxide, zinc phosphate, zinc phosphite, zinc formate, zinc fumarate, zinc sulfide, zinc molybdate, zinc tungstate, zinc oxide, zinc alloys such as zinc-molybdenum alloys.

[0189] In embodiments, the promoter metal is a Group IIA metal compound selected from the group of magnesium, calcium, strontium and barium compounds that is at least partially in the solid state, for example a water-insoluble compound such as a carbonate, hydroxide, fumarate, phosphate, phosphite, sulfide, molybdate, tungstate, oxide, or mixtures thereof.

[0190] In one embodiment, the promoter metal compound is an at least partially solid tin compound, for example a poorly water-soluble tin compound such as stannic acid, tin phosphate, tin formate, tin acetate, tin molybdate, tin tungstate, tin oxide, tin alloys such as tin-molybdenum alloys.

[0191] VIB Group Metal Component: VIB Group Metal (M VIB ) The compound may be added in solid state, partially dissolved state or solution state. In one embodiment, the VIB Group metal compound is selected from molybdenum, chromium, tungsten compounds and combinations thereof. Examples of such compounds include, but are not limited to, alkali metal, alkaline earth metal or ammonium metal salts of molybdenum, tungsten or chromium (e.g., ammonium tungstate, meta-, para-, hexa- or polytungstates, ammonium chromate, ammonium molybdate, iso-, peroxy-, di-, tri-, tetra-, hepta-, octa- or tetradeca-molybdates, alkali metal heptamolybdates, alkali metal orthomolybdates, or alkali metal isomolybdates), ammonium salts of phosphomolybdic acid, ammonium salts of phosphotungstic acid, ammonium salts of phosphochromic acid, (di- and tri-) molybdenum oxide, (di- and tri-) tungsten oxide, chromium oxide, chromic oxide, molybdenum carbide, molybdenum nitride, aluminum molybdate, molybdic acid, chromic acid, tungstic acid, Mo-P heteropolyanion compounds, Wo-Si heteropolyanion compounds, WP heteropolyanion compounds, W-Si heteropolyanion compounds, Ni-Mo-W heteropolyanion compounds, Co-Mo-W heteropolyanion compounds, or mixtures thereof, added in the solid, partially dissolved or solute state.

[0192] Chelating agent (ligand) L: In one embodiment, the catalyst precursor composition comprises at least one non-toxic organic oxygen-containing ligand having an LD50 greater than 500 mg / kg (single oral dose in rats). In a second embodiment, the organic oxygen-containing ligand L has an LD50 of >700 mg / kg. In a third embodiment, the organic oxygen-containing chelating agent has an LD50 of >1000 mg / kg. As used herein, the term "non-toxic" means that the ligand has an LD50 greater than 500 mg / kg (single oral dose in rats). As used herein, the term "at least one organic oxygen-containing ligand" means that in some embodiments, the composition may have more than one organic oxygen-containing ligand, and some organic oxygen-containing ligands may have an LD50 of <500 mg / kg, while at least one organic oxygen-containing ligand has an LD50 of >500 mg / kg.

[0193] In one embodiment, the oxygen-containing chelating agent L is selected from the group of non-toxic organic acid addition salts, such as: formic acid, acetic acid, propionic acid, maleic acid, fumaric acid, succinic acid, tartaric acid, citric acid, oxalic acid, glyoxylic acid, aspartic acid, alkyl sulfonic acids such as methanesulfonic acid and ethanesulfonic acid, aryl sulfonic acids such as benzenesulfonic acid and p-toluenesulfonic acid, and aryl carboxylic acids such as benzoic acid. In one embodiment, the oxygen-containing chelating agent L is maleic acid (LD50 is 708 mg / kg).

[0194] In another embodiment, the non-toxic chelating agent L is selected from the group consisting of glycolic acid (having an LD50 of 1950 mg / kg), lactic acid (LD50 of 3543 mg / kg), tartaric acid (LD50 of 7500 mg / kg), malic acid (LD50 of 1600 mg / kg), citric acid (LD50 of 5040 mg / kg), gluconic acid (LD50 of 10380 mg / kg), methoxyacetic acid (LD50 of 3200 mg / kg), ethoxyacetic acid (LD50 of 1292 mg / kg), malonic acid (LD50 of 1310 mg / kg), succinic acid (LD50 of 500 mg / kg), fumaric acid (LD50 of 10700 mg / kg), and glyoxylic acid (LD50 of 3000 mg / kg). In yet another embodiment, the non-toxic chelating agent is selected from the group of organic sulfur compounds, including but not limited to mercaptosuccinic acid (LD50 of 800 mg / kg) and thiodiglycolic acid (LD50 of 500 mg / kg).

[0195] In yet another embodiment, the oxygen-containing ligand L is a compound containing a carboxylate. In one embodiment, the carboxylate compound contains one or more carboxylate functional groups. In yet another embodiment, the carboxylate compound includes: monocarboxylates, including but not limited to formates, acetates, propionates, butyrates, valerates, and caproates, and dicarboxylates, including but not limited to oxalates, malonates, succinates, glutarates, adipates, malates, maleates, fumarates, and combinations thereof. In a fourth embodiment, the carboxylate compound includes maleates.

[0196] The organic oxygen-containing ligand may be mixed with a solution or mixture containing a promoter metal, a solution or mixture containing a Group VIB metal, or a precipitate, solution, or mixture containing a combination of a promoter metal and a Group VIB metal. The organic oxygen-containing ligand may be in a solution state, wherein the entire amount of the organic oxygen-containing ligand is dissolved in a liquid such as water. During mixing with one or more promoter metals, one or more Group VIB metals, and combinations thereof, the organic oxygen-containing ligand may be partially dissolved and partially in a solid state.

[0197] Diluent Component: The term "diluent" is used interchangeably with "binder." A diluent is optionally used in preparing the catalyst precursor.

[0198] In one embodiment, a diluent is included in the method for preparing a catalyst precursor composition. Typically, the diluent material to be added has a lower catalytic activity or no catalytic activity than a catalyst prepared from a catalyst precursor composition (without a diluent). In one embodiment, the activity of the catalyst may be reduced by adding a diluent. Therefore, in this method, the amount of diluent to be added generally depends on the desired activity of the final catalyst composition. Depending on the envisioned catalytic application, a diluent amount of 0-95% by weight of the total composition may be suitable.

[0199] The diluent may be added simultaneously or sequentially to one or more promoter metal components, a mixture containing promoter metals, a mixture containing one or more VIB Group metals or metals. Alternatively, the promoter metal and the VIB Group metal mixture may be combined together, and the diluent may then be added to the combined metal mixture. It is also possible to combine portions of the metal mixture simultaneously or sequentially, then add the diluent and finally add the remainder of the metal mixture simultaneously or sequentially. In addition, the diluent may also be combined with the metal mixture in the solute state, and then add the metal compound at least partially in the solid state. An organic oxygen-containing ligand is present in at least one metal-containing mixture.

[0200] In one embodiment, the diluent is composited with the Group VIB metal and / or the promoter metal prior to composited with the bulk catalyst precursor composition and / or subsequently added during preparation of the bulk catalyst precursor composition. In one embodiment, composited with any of these metals is by impregnating the solid diluent with these materials.

[0201] Diluent materials include any material commonly used as a diluent or binder in hydroprocessing catalyst precursors. Examples include silica, silica-alumina, such as conventional silica-alumina, silica-coated alumina and alumina-coated silica, alumina such as (pseudo) boehmite, or gibbsite, titania, zirconia, cationic clays or anionic clays such as saponite, bentonite, kaolin, sepiolite or hydrotalcite, or mixtures thereof. In one embodiment, the binder material is selected from: silica, aluminum-doped colloidal silica, silica-alumina, alumina, titania, zirconia, or mixtures thereof.

[0202] These diluents can be applied as such or after peptization. Precursors of these diluents which are converted into any of the above diluents during the process can also be applied. Suitable precursors are, for example: alkali metal aluminates or ammonium aluminates (to obtain alumina diluents), water glass, or ammonium stabilized or acid stabilized silica sols (to obtain silica diluents), mixtures of aluminates and silicates (to obtain silica alumina diluents), mixtures of di-, tri- and / or tetravalent metal sources such as mixtures of water-soluble salts of magnesium, aluminum and / or silicon (to prepare cationic clays and / or anionic clays), aluminum chlorohydroxide (chlorohydrol), aluminum sulfate, or mixtures thereof.

[0203] Other optional components: If necessary, in addition to the above components, other materials (including other metals) can be added. These materials include any materials added during the preparation of conventional hydroprocessing catalyst precursors. Suitable examples are phosphorus compounds, boron compounds, additional transition metals, rare earth metals, fillers, or mixtures thereof. Suitable phosphorus compounds include ammonium phosphate, phosphoric acid or organic phosphorus compounds. The phosphorus compound can be added at any stage of the method steps. Suitable additional transition metals that can be added to the method steps include, for example, rhenium, ruthenium, rhodium, iridium, chromium, vanadium, iron, cobalt, nickel, zinc, platinum, palladium, cobalt, etc. In one embodiment, the additional metal is applied in the form of a water-insoluble compound. In another embodiment, the additional metal is added in the form of a water-soluble compound. In addition to adding these metals during the method, the final catalyst precursor composition can also be compounded with optional materials. For example, the final catalyst precursor composition can be impregnated with an impregnation solution containing any of these additional materials.

[0204] Methods of preparing hydroprocessing catalyst precursors: The preparation methods allow the composition and structure of the catalyst precursor to be systematically varied by controlling the relative amounts of elements, the types of reagents, and the duration and severity of the individual reactions and reaction steps.

[0205] The order of addition of the reagents used to form the catalyst precursor is not important. For example, an organic oxygen-containing ligand can be combined with a mixture of one or more promoter metals and one or more VIB Group metals and then precipitated or co-gelled. An organic oxygen-containing ligand can be mixed with a solution of a promoter metal and then added to a solution of one or more VIB Group metals. An organic oxygen-containing ligand can be mixed with a solution of one or more VIB Group metals and added to a solution of one or more promoter metals.

[0206] Forming a precipitate or cogel with a VIB Group metal / promoter metal: In one embodiment of the method, the first step is a precipitation or cogel step, which includes reacting in a mixture of one or more promoter metal components in solution and a VIB Group metal component in solution to obtain a precipitate or cogel. The precipitation or cogel is carried out at a temperature and pH at which the promoter metal compound and the VIB Group metal compound precipitate or form a cogel. Then, an organic oxygen-containing ligand in solution or at least partially in solution is combined with the precipitate or cogel to form an embodiment of the catalyst precursor.

[0207] In an embodiment, the temperature at which the catalyst precursor is formed is 50-150°C. If the temperature is below the boiling point of the protic liquid (such as 100°C in the case of water), the process is typically carried out at atmospheric pressure. Above this temperature, the reaction is typically carried out at elevated pressure (such as in an autoclave). In one embodiment, the catalyst precursor is formed at a pressure of 0 to 3000 psig. In a second embodiment, the pressure is 100 to 1000 psig.

[0208] Depending on the desired properties of the product, the pH of the mixture can be changed to increase or decrease the rate of precipitation or cogelation. In one embodiment, the mixture maintains its natural pH during one or more reaction steps. In another embodiment, the pH is maintained at 0-12. In another embodiment, the pH is 4-10. In another embodiment, the pH is 7-10. The pH can be increased or decreased by adding a base or acid to the reaction mixture or adding hydroxide ions or H ions that decompose at elevated temperatures to increase or decrease the pH, respectively. + Examples include urea, nitrites, ammonium hydroxide, inorganic acids, organic acids, inorganic bases, and organic bases.

[0209] In one embodiment, the reaction of one or more promoter metal components is carried out using water-soluble metal salts (e.g., zinc, molybdenum, and tungsten metal salts). The solution may also contain other one or more promoter metal components, such as cadmium compounds or mercury compounds such as Cd(NO3)2 or (CH3CO2)2Cd; Group VIII metal components, including cobalt compounds or iron compounds such as Co(NO3)2 or (CH3CO2)2Co; and other one or more Group VIB metal components such as chromium.

[0210] In one embodiment, the reaction of one or more promoter metal components is carried out using water-soluble tin, molybdenum and tungsten metal salts. The solution may also contain other one or more Group IVA metal components, for example lead compounds such as Pb(NO3)4 or (CH3CO2)2Pb, and other Group VIB metal compounds such as chromium compounds.

[0211] The reaction is carried out using appropriate metal salts to produce a precipitate or co-gel combination of zinc / molybdenum / tungsten, tin / molybdenum / tungsten, zinc / molybdenum, zinc / tungsten, tin / molybdenum, tin / tungsten, or zinc / tin / molybdenum / tungsten, or nickel / molybdenum / tungsten, cobalt / molybdenum / tungsten, nickel / molybdenum, nickel / tungsten, cobalt / molybdenum, cobalt / tungsten, or nickel / cobalt / molybdenum / tungsten. The organic oxygen-containing ligand may be added before or after the precipitation or co-gel of the promoter metal compound and / or the VIB Group metal compound.

[0212] The metal precursors may be added to the reaction mixture in the form of a solution, suspension, or a combination thereof. If the soluble salts are added as is, they will dissolve in the reaction mixture and subsequently precipitate or co-gel. The solution may optionally be heated under vacuum to effect precipitation and evaporate the water.

[0213] After precipitation or cogelation, the catalyst precursor may be dried to remove water. Drying may be carried out under atmospheric conditions or in an inert atmosphere such as nitrogen, argon or under vacuum. Drying may be carried out at a temperature sufficient to remove water but not organic compounds. Preferably, drying is carried out at about 120° C. until a constant weight of the catalyst precursor is reached.

[0214] Formation of a precipitate using one or more optional binder components: In one embodiment using a binder, the binder component can be added to a reaction mixture containing a metal precursor in the form of a solution, a suspension, or a combination thereof to form a precipitate or a cogel. The precipitate is then dried to remove water.

[0215] In one embodiment using magnesium aluminum silicate clay as a binder, a first reaction mixture comprising a silicon component, an aluminum component, a magnesium component, a promoter metal compound, and / or a VIB Group metal compound is formed. In one embodiment, the first reaction mixture is formed under ambient pressure and temperature conditions. In one embodiment, the reaction is conducted at a pressure of 0.9 bar to 1.2 bar and a temperature of about 0° C. to 100° C.

[0216] Examples of silicon components include, but are not limited to, sodium silicate, potassium silicate, silica gel, silica sol, hydronium ion stabilized or ammonium stabilized silica sol, and combinations thereof. Examples of aluminum components that can be used in the method of the present invention include, but are not limited to, sodium aluminate, potassium aluminate, aluminum sulfate, aluminum nitrate, and combinations thereof. Examples of magnesium components that can be used in the method of the present invention include, but are not limited to, magnesium metal, magnesium hydroxide, magnesium halide, magnesium sulfate, and magnesium nitrate. In one embodiment, a sufficient amount of acid is added to the mixture containing the metal precursor and the binder component to adjust the pH of the mixture to about 1 to about 6, thereby forming a first reaction mixture.

[0217] After forming the first reaction mixture, a base is added to form a second reaction mixture. Examples of bases include, but are not limited to, ammonium hydroxide, sodium hydroxide, and potassium hydroxide. Sufficient base is added to the first reaction mixture so that the pH of the resulting second reaction mixture is from about 7 to about 12. Then, the second reaction mixture is reacted at a sufficient temperature for a sufficient time to form a catalyst precursor incorporating at least one clay as a binder. In an embodiment, the time is at least 1 second. In a second embodiment, the time is 15 minutes. In a third embodiment, the time is at least 30 minutes. The temperature of the second reaction mixture may be from about 0°C to about 100°C. The reaction may be carried out at ambient pressure, but higher or lower pressures are not excluded.

[0218] In one embodiment using magnesium aluminum silicate clay as a binder, the ratio of silicon to aluminum to magnesium can be expressed as the elemental molar ratio aSi:bAl:cMg, where the "a" value is 3 to 8, the "b" value is 0.6 to 1.6, and the "c" value is 3 to 6.

[0219] Characterization of Catalyst Precursors: Characterization of charge-neutral catalyst precursors can be performed using techniques known in the art, including but not limited to powder x-ray diffraction (PXRD), elemental analysis, surface area measurements, average pore size distribution, average pore volume. Porosity and surface area measurements can be performed using BJH analysis under BET nitrogen adsorption conditions.

[0220] Characteristics of the catalyst precursor: In one embodiment, the catalyst precursor has an average pore volume of 0.05-5 mL / g as measured by nitrogen adsorption. In another embodiment, the average pore volume is 0.1-4 mL / g. In a third embodiment, the average pore volume is 0.1-3 mL / g.

[0221] In one embodiment, the catalyst precursor has at least 10 m 2 In a second embodiment, the catalyst precursor has a surface area of ​​at least 50 m 2 In a third embodiment, the catalyst precursor has a surface area of ​​at least 150 m 2 / g of surface area.

[0222] In one embodiment, the catalyst precursor has an average pore size defined by nitrogen adsorption of 2-50 nanometers. In a second embodiment, the catalyst precursor has an average pore size of 3-30 nanometers. In a third embodiment, the catalyst precursor has an average pore size of 4-15 nanometers.

[0223] In one embodiment comprising a magnesium aluminum silicate clay as a binder, the catalyst precursor is a layered material composed of stacked elemental clay platelets.

[0224] Forming process: In one embodiment, the catalyst precursor composition can be directly formed into various shapes, generally depending on the intended commercial use. These shapes can be made by any suitable technique such as extrusion, pelletization, crimping, or spray drying. If the liquid content of the bulk catalyst precursor composition is too high so that it cannot be directly subjected to the forming step, a solid-liquid separation can be performed before forming.

[0225] Addition of pore formers: The catalyst precursor may be mixed with pore formers including, but not limited to, stearic acid, polyethylene glycol polymers, carbohydrate polymers, methacrylates, and cellulosic polymers. For example, the dried catalyst precursor may be mixed with a cellulose-containing material such as methylcellulose, hydroxypropylcellulose, or other cellulose ethers at a ratio of 100:1 to 10:1 (catalyst precursor weight %: cellulose weight %), and water is added until a mixture having an extrudable consistency is obtained. Examples of commercially available cellulose-based pore formers include, but are not limited to: METHOCEL TM (available from DuPont), (available from DuPont), and Porocel (available from Evonik). The extrudable mixture may be extruded and then optionally dried. In one embodiment, drying may be performed in an inert atmosphere such as nitrogen, argon, or under vacuum. In another embodiment, drying may be performed at an elevated temperature of 70 to 200°C. In yet another embodiment, drying is performed at 120°C.

[0226] Sulfiding agent component: The electrically neutral catalyst precursor can be sulfided to form an active catalyst. In one embodiment, the sulfiding agent is elemental sulfur itself. In another embodiment, the sulfiding agent is a sulfur-containing compound that can decompose into hydrogen sulfide under common conditions. In yet a third embodiment, the sulfiding agent is H2S itself or H2S in H2.

[0227] In one embodiment, the sulfiding agent is selected from the group consisting of ammonium sulfide, ammonium polysulfide ((NH4)2S x ), ammonium thiosulfate ((NH4)2S2O3), sodium thiosulfate (Na2S2O3), thiourea (NH2CSNH2), carbon disulfide, dimethyl disulfide (DMDS), dimethyl sulfide (DMS), mercaptans, di-tert-butyl polysulfide (TBPS), tert-nonyl polysulfide (TNPS), and the like. In another embodiment, the sulfiding agent is selected from alkali metal sulfides and / or alkaline earth metal sulfides, alkali metal hydrogen sulfide and / or alkaline earth metal hydrogen sulfide, and mixtures thereof. The use of a sulfiding agent containing an alkali metal and / or alkaline earth metal may require an additional separation step to remove the alkali metal and / or alkaline earth metal from the spent catalyst.

[0228] In one embodiment, the sulfiding agent is ammonium sulfide in an aqueous solution, which can be synthesized from hydrogen sulfide and ammonia refinery off-gas. Such synthesized ammonium sulfide is readily soluble in water and can be easily stored in a tank in the form of an aqueous solution before use. In one embodiment, the sulfiding is performed using an aqueous solution of ammonium sulfide and also in the presence of at least one sulfur additive selected from the group consisting of thiadiazoles, thioacids, thioamides, thiocyanates, thioesters, thiophenols, thiosemicarbazides, thioureas, mercaptoalcohols, and mixtures thereof.

[0229] In one embodiment, the sulfidation of the catalyst precursor is performed using a hydrocarbon feedstock as a sulfur source.Sulfidation of the catalyst precursor with a hydrocarbon feedstock may be performed during hydroprocessing in one or more hydroprocessing reactors.

[0230] In one embodiment, the sulfiding agent is present in an amount in excess of the stoichiometric amount required to form the sulfided catalyst from the catalyst precursor. In another embodiment, the amount of sulfiding agent represents a molar ratio of sulfur to Group VIB metal of at least 3:1 to produce the sulfided catalyst from the catalyst precursor. In a third embodiment, the total amount of sulfur-containing compound is typically selected to correspond to any of about 50-300%, 70-200%, and 80-150% of the stoichiometric amount of sulfur required to convert the metal to, for example, Co9S8, MoS2, WS2, Ni3S2, etc.

[0231] Sulfiding step: Sulfiding of the catalyst precursor (sometimes referred to as "presulfiding") to form the catalyst (thus ex-situ sulfiding) may be performed prior to introducing the catalyst into the hydroprocessing reactor. In another embodiment, the sulfiding is in-situ. In one embodiment where the sulfiding process is performed ex-situ, the formation of undesirable compounds in the hydroprocessing unit is prevented. In one embodiment, the catalyst precursor is converted into an active catalyst after contacting the catalyst precursor with a sulfiding agent at a temperature of 70°C to 500°C and under a H2-containing gas pressure for 10 minutes to 15 days. If the sulfiding temperature is below the boiling point of the sulfiding agent (such as 60-70°C in the case of ammonium sulfide solution), the process is typically carried out at atmospheric pressure. In the case of a temperature above the boiling temperature of the sulfiding agent / optional component, the reaction is typically carried out at elevated pressure.

[0232] In one embodiment, sulfidation can be carried out in the gas phase using hydrogen and sulfur-containing compounds that can be decomposed into H2S. Examples include mercaptans, CS2, thiophene, DMS, DMDS, and suitable refinery off-gas containing S. It is sufficient to use only H2S. The contact of the catalyst precursor with hydrogen and sulfur-containing compounds in the gas phase can be carried out in one step at a temperature of 125°C to 450°C (257°F to 842°F) in one embodiment and at 225°C to 400°C (437°F to 752°F) in another embodiment. In one embodiment, sulfidation is carried out in a certain period of time at a temperature increase (e.g., 0.5 to 4°C (0.9 to 7.2°F) / min) and maintained for a certain period of time (e.g., 1 to 12 hours) until completion.

[0233] As used herein, completion of the sulfidation process means that at least 95% of the stoichiometric amount of sulfur necessary to convert the metal to, for example, Co9S8, MoS2, WS2, Ni3S2, etc., has been used up.

[0234] In another embodiment of sulfurization in gas phase, sulfurization is carried out in two or more steps, wherein the first step is lower than the temperature of subsequent one or more steps. For example, the first step is about 100 to 250 ℃ (212 ℉ to 482 ℉), preferably about 125 to 225 ℃ (257 ℉ to 437 ℉). After a short period of time of, for example, 0.5 to 2 hours, the temperature remains stable. The second step can be carried out at about 225 to 450 ℃ (437 ℉ to 842 ℉) and preferably about 250 to 400 ℃ (482 ℉ to 752 ℉). The total pressure during the sulfurization step can be normal pressure to about 10 bar (1MPa). In the step, H2 and the gaseous mixture of sulfur-containing compounds can be the same or different. Sulfidation in gas phase can be carried out in any suitable manner, including fixed bed process and moving bed process (wherein the catalyst moves relative to the reactor, such as boiling process and converter).

[0235] In one embodiment, the sulfidation is carried out in the liquid phase. First, the catalyst precursor is contacted with an organic liquid in an amount of 20-500% of the pore volume of the catalyst precursor. The contact with the organic liquid can be carried out at a temperature ranging from room temperature to 250°C (482°F). After the organic liquid is incorporated, the catalyst precursor is contacted with hydrogen and a sulfur-containing compound.

[0236] In one embodiment, the organic liquid has a boiling range of about 100-550°C (212-1022°F). In another embodiment, the organic liquid is a petroleum fraction such as heavy oil, a lubricating oil fraction such as mineral lubricating oil, atmospheric gas oil, vacuum gas oil, straight run gas oil, white solvent oil, middle distillates such as diesel, jet fuel and heating oil, naphtha and gasoline. In one embodiment, the organic liquid contains less than 10% by weight, and preferably less than 5% by weight, sulfur.

[0237] In one embodiment, the vulcanization (or "start-up") in the liquid phase is carried out as a "rapid" process, wherein the vulcanization is carried out in a period of less than 72 hours and with a temperature increase of 0.5 to 4°C (0.9 to 7.2°F) / min. In a second embodiment, the rapid start-up is less than 48 hours. In a third embodiment, the rapid start-up is less than 24 hours.

[0238] In rapid sulfidation, the contact of the catalyst precursor with hydrogen and sulfur-containing compounds in an organic liquid can be carried out in one step at a temperature of 150 to 450°C in one embodiment and at 225°C to 400°C in another embodiment. In another embodiment of rapid sulfidation, sulfidation is carried out in two or more steps, wherein the first step is carried out at a lower temperature than one or more subsequent steps. For example, the first step is carried out at about 100 to 250°C (212°F to 482°F) or 125 to 225°C (257°F to 437°F). After a short period of time of, for example, 0.5 to 2 hours (temperature remains stable), the second step temperature is then increased, for example, to 250 to 450°C (482°F to 842°F), and preferably to 225 to 400°C (437°F to 7520°F). The temperature is maintained for 1 to 36 hours, after which the sulfidation is completed.

[0239] In another embodiment, the sulfidation in the liquid phase is carried out in a "slow" process, wherein the sulfidation is carried out in four days to three weeks at most (i.e., within a time period of at least 96 hours). In this slow process, the contact of the catalyst precursor with hydrogen and sulfur-containing compounds in an organic liquid is carried out in two or more steps, wherein the first step is lower than the subsequent one or more steps, and wherein the temperature is slowly (e.g., per hour) increased, rather than increased per minute as in a quick start. In the step, the gaseous mixture of H2 and sulfur-containing compounds may be the same or different. In one embodiment, the first step is carried out at about 100 to 375°C (212°F to 707°F), preferably about 125 to 350°C (257°F to 662°F), wherein the temperature rise rate is 0.25 to 4°C (0.45 to 7.2°F) / hour. After the first step, the temperature is kept constant for a time period of 2 to 24 hours, and then the second step is increased at a rate of 5 to 20°C (9 to 36°F) / hour. In one embodiment, the second step is conducted at about 200 to 450°C (392°F to 842°F), and preferably about 225 to 400°C (437°F to 752°F).

[0240] In one embodiment, the sulfiding is carried out with elemental sulfur, wherein the sulfur is incorporated into the pores of the catalyst precursor. In this process, the elemental sulfur is mixed with the catalyst precursor in an amount of 2 to 15 weight percent of the weight of the catalyst precursor at a temperature below the melting point of the sulfur. In one embodiment, the mixing is carried out at 180 to 210°F (82°C to 99°C). Sequentially or simultaneously with mixing the precursor with the elemental sulfur, the mixture is contacted with a high boiling point organic liquid. The mixture is then heated to a temperature of 250 to 390°F (121°C to 199°C) in the presence of nitrogen, thereby producing H2S and metal sulfides. In one embodiment, the organic liquid is selected from the group consisting of olefins, gasoline, white solvent oil, diesel, gas oil, mineral lubricating oil, and white oil.

[0241] In one embodiment, it was found that catalysts sulfided from embodiments of the catalyst precursor unexpectedly produced about the same 700°F+ conversion whether sulfided via gas phase or in the liquid phase in a "fast" process. In one embodiment, it was found that the 700°F+ conversion was improved by at least 25% using a catalyst sulfided in the liquid phase and via a "slow" process. In yet another embodiment, the 700°F+ conversion was doubled using a catalyst sulfided via a slow process.

[0242] In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum and tungsten. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten and titanium. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten and niobium. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten, niobium and titanium. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten, niobium and titanium. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten, niobium and copper. In certain embodiments, the self-supported hydroprocessing catalyst comprises nickel, molybdenum, tungsten and copper.

[0243] In certain embodiments, the self-supported hydroprocessing catalyst comprises about 5 to about 9 weight percent molybdenum, about 21 to 31 weight percent nickel, and about 33 to about 42 weight percent tungsten. In certain embodiments, the self-supported hydroprocessing catalyst comprises about 5.9 to about 8.1 weight percent molybdenum, about 21.8 to 30.7 weight percent nickel, and about 34.4 to about 41.3 weight percent tungsten.

[0244] The preferred catalyst precursor is Ni-Mo-W maleate catalyst precursor. The catalyst is preferably sulfided with dimethyl sulfide (DMDS).

[0245] In certain embodiments, the self-supported hydroprocessing catalyst is a catalyst comprising nickel, molybdenum, and tungsten, such as ICR 1000, ICR 1001, ICR 1003, and ICR4000 (all available from Advanced Refining Technologies LLC).

[0246] In certain embodiments, the self-supported hydroprocessing catalyst layer comprises or consists of one type of self-supported hydroprocessing catalyst.In certain embodiments, the self-supported hydroprocessing catalyst layer comprises or consists of two types of hydrocracking catalysts.

[0247] Hydrocarbon feedstock

[0248] A variety of petrochemical feedstocks can be hydroprocessed (hydrotreated) by the layered catalyst reactor system and method. Suitable feedstocks include: whole fraction crude oils and reduced petroleum crudes; atmospheric and vacuum residues; propane deasphalted residues such as brightstock, cycle oils, FCC bottoms; gas oils, including atmospheric and vacuum gas oils and coker gas oils; light to heavy distillates, including crude virgin distillates; hydrocracked products; hydrotreated oils; dewaxed oils; slack waxes; Fischer-Tropsch waxes; raffinates; naphthas; and mixtures of these materials. Typical lighter feeds include fractions boiling at about 175°C (about 350°F) to about 375°C (about 750°F). Using this type of feed, a considerable amount of hydrocracked naphtha is produced, which can be used as a low sulfur gasoline blending stock. Typical heavier feeds include, for example, vacuum gas oils boiling at up to about 593°C (about 1100°F) and typically about 350°C to about 500°C (about 660°F to about 935°F), and in such cases the proportion of diesel fuel produced is correspondingly higher.

[0249] Method for hydrotreating hydrocarbon feedstock

[0250] In one aspect, the present invention relates to a method for hydrotreating a hydrocarbon feedstock, comprising: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen and olefins with a layered catalyst reactor system as described herein in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically through the layers of the layered catalyst reactor system in sequence from top to bottom; and (iii) recovering the hydrocarbon product from the bottom of the layered catalyst reactor system. The method can be used to remove impurities or contaminants such as metals, sulfur and nitrogen from the hydrocarbon feedstock, and to saturate olefins and aromatic compounds. The method is carried out under conditions that promote hydrodemetallization, hydrodesulfurization and hydrodenitrogenation.

[0251] In embodiments, the method is operated by directing a feedstock containing high levels of sulfur and nitrogen to an initial treatment reaction stage to convert substantial amounts of sulfur and nitrogen in the feed into inorganic forms, with the primary purpose in this step being to reduce the feed nitrogen content. In the presence of hydrogen, a hydrotreating step is performed in an exemplary layered catalyst reactor system. Depending on the feed characteristics, the conditions used are suitable for hydrodesulfurization and / or denitrogenation. The product stream is then transferred to the hydrocracking zone directly (unseparated) or by separation and water washing, where a boiling range conversion is performed. In an exemplary system, the product stream from the first and second layers together with the hydrogen treat gas and other hydrotreating / hydrocracking reaction products including hydrogen sulfide and ammonia can be transferred to a separator, where hydrogen, light fractions, and inorganic nitrogen and hydrogen sulfide are removed from the hydrocracking liquid product stream. The circulating gas can be washed to remove ammonia, and can be subjected to amine washing to remove hydrogen sulfide, thereby improving the purity of the recycled hydrogen and thus reducing the product sulfur content.

[0252] The product stream then continues to the hydrocracking layer and the self-supported catalyst layer for processing. In certain embodiments, "hard sulfur" species are removed, i.e., sulfur species having atmospheric boiling points of about 93°C to about 593°C (200°F to about 1100°F), particularly about 350°C to about 500°C (about 660°F to about 935°F).

[0253] Example

[0254] The disclosed embodiments are further illustrated by the following examples, which should not be construed in any way as imposing limitations on the scope of the invention. Various other aspects, embodiments, modifications and equivalents thereof may be apparent to those of ordinary skill in the art after reading the description herein without departing from the scope of the invention.

[0255] Example 1

[0256] This study explored the hydroprocessing of products derived from the LC refining process. Tests were conducted with Arab mid-grade crude based LC Finate material and Urals based feed.

[0257] Bench scale unit (BSU), catalyst system and feed

[0258] Several lab scale units were used for this study (BSU 607, 612 and 911). Several catalyst systems were tested in separate runs, runs 56 to 62 in BSU607, runs 37 to 41 in BSU612 and runs 160 and 161 in BSU911.

[0259] The layered catalyst reactor system used is described in Table 1. Monolithic extrudates shortened to an L / D of 1 to 2 and filled with -100 mesh alundum were used to prevent bypass and channeling. One of the main goals of this study was to evaluate the performance of ICR 1000 / 1001 in upgrading these challenging feeds. Catalyst systems containing about 10% to about 20% ICR 1000 and / or about 14% to about 44% ICR 1001 were explored. Comparative examples include catalyst systems utilizing ICR 183 and ICR 191 as hydrocracking catalysts. ICR 250 is used in combination with ICR 1000 and is typically located in front of (on top of) ICR 1000 or ICR 1001. One comparative example includes a catalyst system containing only ICR 250 (no ICR 1000 or ICR 1001).

[0260] Table 1

[0261]

[0262]

[0263] *LOI = Loss on Ignition

[0264] The feed for most units is vacuum heavy gas oil (HVGO) (ABQ1560) from the LC refining unit and 900-℉ VGO (ABQ1967) derived from this feed. ABQ1560 consists of 75% LC finate HVGO and 25% straight run (SR) HVGO. A blend of ABQ1560 and SRC HVGO (TGQ9588) that achieves a 50% blend of LC refinery product and HVGO is used to evaluate the dilution effect on activity / stability. The additional feeds used were based on Ural derived feeds from RAM (Milazzo Refinery LC Refinery HVGO, TGQ9989), diluted with SRC HVGO to a 50 / 50 blend (CGQ0003); and Neste (Neste LC Refinery Heavier VGO, ABQ1956), diluted with SRC HVGO to a 50 / 50 blend (CGQ0107). The properties of the feeds used are shown in Table 2. The feed sample descriptions are provided in Table 2 below.

[0265] Table 2

[0266]

[0267]

[0268] Feed sample description:

[0269] A = ABQ1560 = HVGO from GS Caltex LC refining unit (25% SR HVGO)

[0270] B = AB1967 = LVGO from ABQ1560 GSC LC Finate 650-900FC = ABQ1214 = SRCVGO blend

[0271] D = TGQ9588 = 50 / 50 blend of GSC LCF VGO and SRC HVGO

[0272] E=TGQ9589=RAM LC Finate VGO

[0273] F = CGQ0003 = 50 / 50 blend of RAM LC Finate VGO and SRC HVGO

[0274] G=ABQ1956=Neste LC Finate heavier VGO

[0275] H = GCGQ0107 / 520 = 50 / 50 blend of Neste LC Finate VGO and SRC HVGO

[0276] Catalyst sulfidation

[0277] The catalyst system was sulfided with VGO doped with DMDS before use:

[0278] - Heat the reactor to 250°F under nitrogen flow (no feed flow, 200 mL / min nitrogen flow) at ambient pressure and hold for one hour;

[0279] -Change to hydrogen at a flow rate of 321 mL / min and increase the pressure to 800 psig;

[0280] -Changed to 13.45 g / h of sulphurized feed (2.5 wt% DMDS in diesel) (LHSV = 1.3 h -1 ), and the hydrogen rate was changed to 255 mL / min (5500 SCF / bbl hydrogen) and maintained for 10 hours;

[0281] - Raise the reactor temperature at 30°F / h to 482°F and hold for 5 hours;

[0282] - Raise the reactor temperature to 572°F at 30°F / h and hold for 5 hours;

[0283] - Raise the reactor temperature to 650°F at 30°F / h and hold for 6 hours;

[0284] -Change to diesel ABQ0920 (LHSV = 0.5h -1 ), raised the pressure to 2350 psig, reduced the hydrogen flow rate to 89.07 mL / min (5000 scf / bbl), and continued for 3 days to de-edge the catalyst.

[0285] Test conditions

[0286] The operating process conditions are:

[0287] 0.40h -1 LHSV (0.50h without demetallization catalyst ICR 132) -1 LHSV) and 0.8h -1 LHSV (1.0h without demetallization catalyst ICR 132) -1 LHSV of

[0288] 2350 psig total pressure (inlet H2 partial pressure is 2250 psi);

[0289] 8000SCFB once through H2;

[0290] - Reactor temperature was 710°F to 765°F to achieve the goal of utilizing different feeds.

[0291] - Two strippers are used in unit 607 / 612 with target distillation temperatures of 300°F and 700°F.

[0292] - A stripping column is used in unit 911 with a target distillation temperature of 700°F.

[0293] The target values ​​for -S were below 100 ppm for the total liquid product (WLP) and below 30 ppm for the diesel fraction (V3O samples) of both stripper units.

[0294] - In WLP, the target value for N is below 40ppm.

[0295] All products (gas, STO, STB or V3O / V3B) were analyzed using SimDist to calculate the output structure.

[0296] The STB or V3O / V3B products were further analyzed for sulfur and nitrogen. Additional analyses were performed for selected production periods.

[0297] These above conditions were chosen as the initial test method for ABQ1560, which is considered to be a very difficult feed. Recent design information for the LC Max hydrotreater / hydrocracker (see EDP CLG Hydrocracking / Hydroprocessing Technology, Shandong Sincier Petrochemical Co Ltd, Volume 1, September 2014) shows different conditions, namely:

[0298] - Reactor inlet pressure was 2200 psi with an average hydrogen partial pressure of 2000 psi.

[0299] - The intake air to oil ratio is less than 5000 SCF / bbl compared to 8000 SCF / bbl in our initial test case.

[0300] -Compared to 0.4 / 0.8h -1 , LHSV is 0.7h -1 .

[0301] - The feed was a blend with a ratio of 45 vol% LC refinery product and 55 vol% SR HVGO.

[0302] - LC refinery HVGO has a distillation EP of 952°F (511°C) with about 22% of the material boiling above 900°F.

[0303] The additional feeds described in Table 2 and subsequently used during this study addressed this issue and brought the feed / reaction conditions closer to the Sincier design.

[0304] Feed conversion is usually performed at two different conditions to estimate the activation energy of HCR / HDN / HDS and calculate the normalized temperature. Temperature normalization is usually performed with a target of 40 ppm nitrogen, 100 ppm sulfur, and 30% hydrocracking to 700-°F fraction.

[0305] Results and discussion

[0306] The operating conditions and test results for completed runs in BSU607-56 to 61, BSU911-160 and 161, and 612-37 to 40 are shown in Tables 3, 4, 5, and 6 (the values ​​shown are averaged over multiple 24 hour production periods).

[0307] Table 3. Operating conditions and test results of comparative examples BSU 607-56, 605-57 and 911-160

[0308]

[0309]

[0310] Table 4. Operating conditions and test results of comparative examples BSU 607-59 and 612-37

[0311]

[0312] Table 5. Operating conditions and test results for comparative example BSUs 612-39 and 607-61 and exemplary example 911-161

[0313]

[0314]

[0315] Table 6. Operating conditions and test results for comparative example BSUs 612-38 and 607-60 and exemplary example 612-40

[0316]

[0317]

[0318] The normalized temperatures for hydrocracking to <700°F fraction (HCR<700°F, 30%), hydrodenitrogenation (HDN, 40 ppm), and hydrodesulfurization (HDS, 100 ppm) are calculated together with the actual reactor temperatures and the calculated activation energies. Figures 1 to 10 Shown in.

[0319] For the heaviest feed ABQ1560, most of which boils at >900°F, stable operation could not be achieved with any catalyst system. Although the base case (no ICR 1000) and 10% ICR 250 / 10% ICR 1000 showed high deactivation of 10°F / 1000 hours ( Figure 1 and 2 ), but the catalyst system utilizing 10% ICR 250 / 20% ICR 1000 showed improved stability (approximately 4°F / 1000 hours, Figure 3 ), which is lost when the ICR 1000 content is increased to 44% ( Figure 4 ). Compared to the base case, the activity advantage using ICR 1000 can be as much as 20℉. Figure 3 The jump in normalized temperature at about 400 h of run time is due to the previous feed loss lasting more than 36 h, which leads to a loss of activity after restart.

[0320] Dilution of ABQ1560 (75 / 25 blend of full range LC Finate VGO and SR HVGO) to a 50 / 50 blend of LC Finate and SR HVGO (TGQ9588) gave a base case stable run on HDN and HDS using ICR 191 (considered to have the same activity as ICR 183). -1 At low LHSV, the required temperature for 40 ppm N and 100 ppm S is 720 to 730°F, but at higher 0.8 h -1 The LHSV increased by more than 30℉( Figure 5 ), which will be closer to the space velocity required to convert this feed.

[0321] At 0.8h -1 Testing a 50 / 50 blend of RAM LC Finate and SR HVGO (i.e., CGQ0003) showed stable performance at an LHSV of more than 15°F ( Figure 6 ), which may be due to the smaller amount of 900+°F material (about 25 wt% in RAM vs. about 50 wt% in GSC feed). Dilution of the LC Finate product is one way to achieve the desired properties.

[0322] ABQ1967 is made from ABQ1560 by distillation to a lower distillation temperature and contains about 15 wt% 900°F+ material with an end point of about 930°F. This feed was tested with the base catalyst system (containing ICR 191) and compared to systems containing 34% and 44% ICR 1000. Using diluted ABQ1560 (612-37, Figure 5 ) and undiluted ABQ1967 (612-39, Fig. 9 ) based system comparison shows that at 0.4h -1 and 0.8h -1 Similar activity and stable performance at LHSV of 1.5 % and 1.2 % respectively, indicating that reducing the 900+℉ content of the feed has a similar effect on the stability / activity of the catalyst system as dilution. Base Case vs. 44% ICR 1000 Case ( Fig.10 ) showed reduced stability for the 44% ICR1000 case with a 10°F activity advantage. We started a run with ABQ1967 on a catalyst system containing 34% ICR 1000 to check if the 44% ICR 1000 had the thermal management issues observed with the ABQ1560 feed (see above).

[0323] The feed closest to the Sincier design conditions is CGQ0107 / CGQ0520, made from a 50 / 50 blend of Neste LCFinate and SRC HVGO. This feed has been tested so far with 34% ICR 1000 and 44% ICR 1000, and is currently being tested with a 55% ICR 250 system without ICR 1000. The difference between the two cases is small, with the 44% ICR 1000 system having a slightly lower activity on HDN. This may also be due to the fact that the 44% ICR 1000 system was first used for ABQ1560 conversion, which showed a high deactivation rate. For both cases, the total sulfur and nitrogen content can be maintained below 40 ppm S and below 30 ppm N, with values ​​as low as 7 ppm N and 15 ppm S in the 726-736°F temperature range (see Table 3).

[0324] The diesel yields for all cases ranged from 13% to 32%, depending on the conversion. Fig.11 It was shown that the diesel yield depends on the feed composition rather than the catalyst system, with RAM based feed showing the highest yield at the same conversion.

[0325] Observations

[0326] 1. The stability of the catalyst system depends on the distillation temperature of LC Finate and the dilution. Dilution to at least a 50 / 50 blend and lowering the end point and overall 900+℉ material improves the activity / stability of the system.

[0327] 2. Addition of ICR 1000 significantly enhanced hydrodenitrogenation (HDN) and hydrodesulfurization (HDS) activities, but no improvement seemed to be shown at higher ICR 1000 contents, as shown by the comparison of the 34% and 44% ICR 1000 cases.

[0328] 3. Without utilizing the ICR 1000, low nitrogen / sulfur levels (<10 ppm / 30 ppm) cannot be achieved at the desired operating start temperature of approximately 730°F.

[0329] 4. For the feeds and catalyst systems studied, the diesel yield (350-700°F range) at the same conversion depends on the feed composition rather than the catalyst system.

Claims

1. A layered catalyst reactor system comprising a vertical bed of catalyst layers arranged from top to bottom in the following order: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) a layer of one or more self-supported hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) a layer of one or more self-supported hydroprocessing catalysts; (vii) a layer of one or more supported hydroprocessing catalysts; wherein the total volume of the two layers comprising one or more self-supported hydroprocessing catalysts is from 10% to less than 44% of the total volume of catalyst in the vertical bed; and The total volume of the two layers comprising one or more supported hydrocracking catalysts is from greater than 10% to 30% of the total volume of the catalyst in the vertical bed.

2. The layered catalyst reactor system of claim 1, wherein the one or more self-supported hydroprocessing catalysts comprise 5 wt% to 9 wt% molybdenum, 21 wt% to 31 wt% nickel, and 33 wt% to 42 wt% tungsten.

3. The layered catalyst reactor system of claim 1, wherein the one or more demetallization catalysts are selected from the group consisting of natural aluminum silicate or synthetic alumina rich in oxides of molybdenum, cobalt and nickel.

4. The layered catalyst reactor system of claim 1, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of a catalyst comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolites, amorphous silica-alumina, and titania-alumina.

5. The layered catalyst reactor system of claim 1, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of catalysts comprising Pd or Pt.

6. The layered catalyst reactor system of claim 1, wherein the one or more hydrocracking catalysts are selected from the group consisting of catalysts comprising nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and nickel-tungsten and / or nickel-molybdenum.

7. The layered catalyst reactor system of claim 1, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material.

8. The layered catalyst reactor system of claim 1, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum, and / or tungsten.

9. A layered catalyst reactor system comprising a vertical bed of catalyst layers arranged from top to bottom in the following order: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) a layer of one or more self-supported hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) a layer of one or more self-supported hydroprocessing catalysts; (vii) a layer of one or more supported hydrocracking catalysts; (viii) a layer of one or more self-supported hydroprocessing catalysts; (ix) a layer of one or more supported hydroprocessing catalysts; wherein the total volume of the three layers comprising one or more self-supported hydroprocessing catalysts is from 9% to less than 44% of the total volume of the catalyst in the vertical bed; and The total volume of the three layers comprising the one or more supported hydrocracking catalysts is from 15% to 30% of the total volume of the catalyst in the vertical bed.

10. The layered catalyst reactor system of claim 9, wherein the one or more self-supported hydroprocessing catalysts comprise 5 wt% to 9 wt% molybdenum, 21 wt% to 31 wt% nickel, and 33 wt% to 42 wt% tungsten.

11. The layered catalyst reactor system of claim 9, wherein the one or more demetallization catalysts are selected from the group consisting of natural aluminum silicate or synthetic alumina rich in oxides of molybdenum, cobalt and nickel.

12. The layered catalyst reactor system of claim 9, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of: catalysts comprising at least one Group VIII metal and at least one Group VIB metal on a support material selected from the group consisting of alumina, zeolites, amorphous silica-alumina, and titania-alumina.

13. The layered catalyst reactor system of claim 9, wherein the one or more supported hydroprocessing catalysts are selected from the group consisting of catalysts comprising Pd or Pt.

14. The layered catalyst reactor system of claim 9, wherein the one or more hydrocracking catalysts are selected from the group consisting of catalysts comprising nickel, nickel-cobalt-molybdenum, cobalt-molybdenum, and nickel-tungsten and / or nickel-molybdenum.

15. The layered catalyst reactor system of claim 9, wherein the one or more hydrocracking catalysts comprise a porous support material comprising a refractory oxide material.

16. The layered catalyst reactor system of claim 9, wherein the one or more hydrocracking catalysts comprise nickel, cobalt, molybdenum, and / or tungsten.

17. A method for hydrotreating a hydrocarbon feedstock, wherein include: (i) contacting a hydrocarbon feedstock containing contaminants including metals, sulfur, nitrogen and olefins with a layered catalyst reactor system in the presence of hydrogen to produce a hydrocarbon product having a lower content of metals, sulfur, nitrogen and olefins than the hydrocarbon feedstock; (ii) passing the hydrocarbon feedstock vertically and sequentially through the layers of the layered catalyst reactor system from top to bottom; and (iii) recovering the hydrocarbon product from the bottom of the layered catalyst reactor system; The layered catalyst reactor system comprises a vertical bed of catalyst layers arranged from top to bottom in the following order: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) a layer of one or more self-supported hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) a layer of one or more self-supported hydroprocessing catalysts; (vii) a layer of one or more supported hydroprocessing catalysts; wherein the total volume of the two layers comprising one or more self-supported hydroprocessing catalysts is from 10% to less than 44% of the total volume of catalyst in the vertical bed; and wherein the total volume of the two layers comprising one or more supported hydrocracking catalysts is greater than 10% to 30% of the total volume of the catalyst in the vertical bed; or The layered catalyst reactor system comprises a vertical bed of catalyst layers arranged from top to bottom in the following order: (i) a layer comprising one or more demetallization catalysts; (ii) a layer of one or more supported hydroprocessing catalysts; (iii) a layer of one or more supported hydrocracking catalysts; (iv) a layer of one or more self-supported hydroprocessing catalysts; (v) a layer of one or more supported hydrocracking catalysts; (vi) a layer of one or more self-supported hydroprocessing catalysts; (vii) a layer of one or more supported hydrocracking catalysts; (viii) a layer of one or more self-supported hydroprocessing catalysts; (ix) a layer of one or more supported hydroprocessing catalysts; wherein the total volume of the three layers comprising one or more self-supported hydroprocessing catalysts is from 9% to less than 44% of the total volume of the catalyst in the vertical bed; and The total volume of the three layers comprising the one or more supported hydrocracking catalysts is from 15% to 30% of the total volume of the catalyst in the vertical bed.

18. The method of claim 17, wherein the layered catalyst reactor system is operated at a temperature of 700°F to 775°F.

19. The process of claim 17, wherein the process has a weight hourly space velocity (WHSV) of 0.4 hr -1 Up to 1.1hr -1 .

20. The process of claim 17, wherein the process has a liquid hourly space velocity (LHSV) of 0.3 hr -1 Up to 0.9hr -1 .

21. The process of claim 17 wherein the normalized temperature of the layered catalyst reactor system is maintained below 770°F during the process.