A high-rebound environmentally friendly TPU shoe midsole and preparation method thereof
Through the composite structure of high-resilience environmentally friendly TPU shoe midsole, combined with specific TPU polymer and polyurethane acrylate polymer, the problem of insufficient hardness and elasticity of TPU shoe midsole is solved, the resilience and shock-absorbing performance are improved, and Enhanced anti-counterfeiting effect.
Patent Information
- Application Number
- CN202410365651.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing TPU shoe midsoles have high hardness and low elasticity, resulting in insufficient resilience and shock-absorbing capabilities when worn, low production efficiency and unstable quality.
A high-resilience environmentally friendly TPU shoe midsole with a composite structure, including a mid-bottom layer and a TPU thick bottom layer bonded by hot melt adhesive. The side of the TPU thick bottom layer away from the mid-bottom layer is coated with an elastic resin layer, and the surface of the elastic resin layer is provided with prefabricated Textured structure and optical coating layer, prepared with specific TPU polymer and polyurethane acrylate polymer to improve mechanical strength and wear resistance.
While maintaining the hardness and durability requirements, it significantly improves the resilience and shock-absorbing performance of the midsole, improves wearing comfort, and enhances anti-counterfeiting performance through optical anti-counterfeiting effects.
Smart Images

Figure CN118021035B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sole materials and production, and in particular to a high-rebound environmentally friendly TPU shoe midsole and a preparation method thereof. Background Art
[0002] The shoe midsole is a shoe material located between the insole and the outsole, and is mainly responsible for providing the elastic cushioning properties and durability of the shoe sole. At present, the main types of shoe midsoles are divided into EVA midsoles, TPU midsoles, air cushion midsoles or woven midsoles, and the types of shoe midsoles are closely related to the elastic cushioning properties and durability of the shoe sole. Among them, the EVA foamed midsole obtained by the EVA foaming process has the characteristics of light texture, excellent shock absorption and rebound, but it is severely worn during long-term use and has poor durability. Most TPU soles are introduced into the cellular structure on the polyurethane matrix through physical foaming, but the process control requirements of the foaming process are high, making it difficult to control the product parameters such as the density, hardness and size of the TPU foaming material, resulting in low production efficiency and unstable quality. At the same time, the traditional TPU shoe midsole has a high hardness and low elasticity, which makes the resilience and shock absorption ability of this type of sole weak when worn, which seriously reduces the wearer's wearing comfort. To this end, the present application proposes a TPU shoe midsole with a composite structure by utilizing the advantages of the EVA midsole and the TPU midsole, so that it has both elastic cushioning and durability. Summary of the invention
[0003] The purpose of the present invention is to solve the above-mentioned deficiencies in the prior art and to provide a high-resilience environmentally friendly TPU shoe midsole and a preparation method thereof.
[0004] The objective of the present invention is achieved through the following technical scheme: a high-rebound, environmentally friendly TPU shoe midsole, the shoe midsole comprising a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot-melt adhesive, and the side of the TPU thick bottom layer away from the mid-bottom layer is coated with an elastic resin layer.
[0005] Furthermore, a prefabricated texture structure is provided on the surface of the elastic resin layer, and an optical coating layer is provided on a side of the elastic resin layer away from the TPU thick bottom layer.
[0006] In practical applications, by setting a prefabricated texture structure and an optical coating layer on the surface of the elastic resin layer, the optical anti-counterfeiting effect of the TPU midsole can be increased, so that the TPU midsole shows a corresponding optical effect under the action of light, and plays an anti-counterfeiting role. Specifically, the prefabricated texture structure is a grating structure, and the grating structure includes a plurality of continuously arranged cylindrical lenses, and the two ends of the cylindrical lenses are respectively connected to the optical coating layer and the TPU thick bottom layer. The optical coating layer is made by depositing a nano-metal film on the surface of the elastic resin layer using electron beam physical vapor deposition technology.
[0007] Furthermore, a pattern layer is provided on one side of the elastic resin layer away from the thick TPU bottom layer, and the pattern layer is formed by printing water-based ink or bio-based ink on the surface of the elastic resin layer to form different colors, texts or patterns and combinations thereof.
[0008] Furthermore, the mid-bottom layer is any one of an EVA mid-bottom layer, a TPU mid-bottom layer or a nylon mid-bottom layer.
[0009] Furthermore, the hot melt adhesive is any one of EVA hot melt adhesive, TPU hot melt adhesive or nylon hot melt adhesive.
[0010] Furthermore, the TPU thick bottom layer is obtained by injecting a heated molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: the polyester polyol and the diisocyanate are fully mixed, the temperature is slowly increased to 70-80°C, a catalyst is added to react for 3-4 hours, a chain extender is added thereto to continue the reaction for 0.5-1h, the temperature is lowered to below 40°C, and then a capping agent is added thereto for capping, and the reaction is stopped after the -NCO group is completely consumed, thereby obtaining the TPU polymer.
[0011] In the above steps, the isocyanate index is 0.99-1.01, the hard segment content is 25-30%, the catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.05-0.15%, the chain extender is polyethylene adipate, and the amount of the chain extender is 20-25% of the total mass of the polyester polyol and the diisocyanate, and the end-capping agent is MPTMS, and the amount of the end-capping agent is 5-10% of the total mass of the polyester polyol and the diisocyanate.
[0012] Furthermore, the preparation step of the polyester polyol is: placing glycolide, caprolactone, 1,4-butanediol and stannous octoate in a reactor and stirring, then raising the temperature to 130-150°C for reaction for 7-9 hours, thereby obtaining the polyester polyol. The molar ratio of glycolide, caprolactone and 1,4-butanediol is 12-15:55-60:26-30, and the amount of stannous octoate is 0.5-2% of the total mass of glycolide, caprolactone and 1,4-butanediol.
[0013] Further, the diisocyanate is mixed with isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 4-6:1, wherein the preparation step of the modified isophorone diisocyanate trimer is as follows: mercaptopropyl trimethoxysilane, isophorone diisocyanate trimer and triethylamine are placed in a reactor and stirred, the temperature is raised to 70-80°C, and the reaction is carried out until the content of the isocyanate group reaches the theoretical target value to obtain the modified isophorone diisocyanate trimer. Specifically, the mass ratio of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer is 1:3-3.5, and the amount of the triethylamine is 0.01-0.05% of the total mass of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer.
[0014] Furthermore, the elastic resin compound comprises the following raw materials in parts by weight: 30-40 parts of polyurethane acrylate polymer, 15-25 parts of epoxy resin, 2-5 parts of photoinitiator, and 20-25 parts of active diluent.
[0015] Furthermore, the elastic resin compound is prepared by weighing polyurethane acrylate polymer and epoxy resin according to the formula ratio, placing them in a reactor at room temperature, and then adding a photoinitiator and a reactive diluent and mixing them thoroughly to obtain the elastic resin compound.
[0016] Furthermore, the photoinitiator is at least one of triphenyl hexafluoroantimonate, ethyl 2,4,6-trimethylbenzoylphosphonate or Irgacure 2959; the diluent is at least one of 4-vinyl cyclohexene oxide, butyl acrylate or 1,6-hexanediol diacrylate.
[0017] Furthermore, the preparation method of the polyurethane acrylate polymer comprises the following steps:
[0018] (1) placing polytetramethylene glycol, about 1 / 4 of a catalyst and a small amount of solvent in a reactor at a temperature of 60-65° C., and then slowly adding isophorone diisocyanate dropwise thereto for a reaction of 2 hours;
[0019] (2) Add about 1 / 4 of the catalyst, chain extender and a small amount of solvent into the reactor and continue the reaction for 2 hours;
[0020] (3) adding butyl 4-hydroxyacrylate and the remaining catalyst to the reactor, raising the temperature to 70-80° C., and reacting for 2-3 hours to obtain a prepolymer solution;
[0021] (4) placing the prepolymer solution obtained in step (3) at 80-90° C. to evaporate the solvent, thereby obtaining a polyurethane acrylate polymer.
[0022] In the preparation of the above-mentioned polyurethane acrylate polymer, the molar ratio of the polytetramethylene ether diol to isophorone diisocyanate is 1:3; the molar amount of the catalyst is 0.5-2% of the molar amount of the polytetramethylene ether diol; the molar ratio of the 1-hydroxybutyl acrylate to the polytetramethylene ether diol is 2:1; and the solvent is N,N-dimethylformamide.
[0023] In the present invention, the polyurethane acrylate polymer prepared by the above steps has a high content of flexible segments, which gives the polyurethane acrylate polymer good flexibility, elasticity and wear resistance. The elastic resin sizing material uses the polyurethane acrylate polymer as the main raw material, adds epoxy resin to compensate for its strength, and enhances the bonding performance and high temperature resistance, and improves the curing efficiency and degree of the reaction system through the photoinitiator.
[0024] The present invention also provides a method for preparing a high-resilience environmentally friendly TPU shoe midsole, comprising the following preparation steps:
[0025] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0026] S2, coating the front side of the thick TPU bottom layer with elastic resin rubber, and curing it with UV light to form an elastic resin layer;
[0027] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0028] Furthermore, the preparation method further comprises: in step S2, using an embossing roller to roll the elastic resin layer at a pressure of 400-600 kPa, so that the elastic resin layer is formed with a prefabricated texture structure.
[0029] Furthermore, the preparation method further comprises: in step S2, using water-based ink or bio-based ink to print different colors, patterns or texts and combinations thereof on the surface of the elastic resin layer to form a pattern layer.
[0030] Furthermore, the UV light energy density emitted by the UV machine is 800-1000mW / cm 2 .
[0031] The beneficial effects of the present invention are:
[0032] (1) The TPU polymer of the present invention uses specific polyester polyols and diisocyanates as raw materials, wherein isophorone diisocyanate and modified diisocyanate trimer are used as hard segments, and polysiloxane is grafted on the side chain of TPU, which can significantly improve the mechanical strength, wear resistance, and water resistance, light resistance and heat resistance stability of the TPU polymer;
[0033] (2) The present invention uses polyurethane acrylate polymer and epoxy resin as raw materials, wherein the polyurethane acrylate polymer has a high content of flexible segments, which gives the polyurethane acrylate polymer good flexibility, elasticity and wear resistance; the addition of epoxy resin can improve its strength, bonding performance and high temperature resistance, and the photoinitiator improves the curing efficiency and degree of the reaction system;
[0034] (3) The present invention adopts a composite structure of a midsole, hot melt adhesive, a TPU thick bottom layer and an elastic resin layer, which not only maintains the hardness and durability requirements of the TPU midsole, but also gives the midsole resilience and shock absorption performance, thereby significantly improving the wearing comfort of the midsole. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a product diagram of the present invention;
[0036] Figure 2 yes Figure 1 A partial enlarged view of . DETAILED DESCRIPTION
[0037] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0038] As a classic embodiment of the present invention, a high-resilience environmentally friendly TPU shoe midsole comprises a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot melt adhesive, and a side of the TPU thick bottom layer away from the mid-bottom layer is coated with an elastic resin layer, wherein the thickness of the TPU thick bottom layer is 0.1-0.2 mm.
[0039] Optionally, according to actual conditions, a prefabricated texture structure is provided on the surface of the elastic resin layer, and an optical coating layer is provided on a side of the elastic resin layer away from the TPU thick bottom layer.
[0040] Optionally, according to actual conditions, a pattern layer is provided on one side of the elastic resin layer away from the TPU thick bottom layer, and the pattern layer is printed on the surface of the elastic resin layer by water-based ink or bio-based ink to form different colors, texts or patterns and combinations thereof.
[0041] Furthermore, the mid-bottom layer is any one of an EVA mid-bottom layer, a TPU mid-bottom layer or a nylon mid-bottom layer.
[0042] Furthermore, the hot melt adhesive is any one of EVA hot melt adhesive, TPU hot melt adhesive or nylon hot melt adhesive.
[0043] Furthermore, the TPU thick bottom layer is obtained by injecting a heated molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: the polyester polyol and the diisocyanate are fully mixed, the temperature is slowly increased to 70-80°C, a catalyst is added to react for 3-4 hours, a chain extender is added thereto to continue the reaction for 0.5-1h, the temperature is lowered to below 40°C, and then a capping agent is added thereto for capping, and the reaction is stopped after the -NCO group is completely consumed, thereby obtaining the TPU polymer.
[0044] Furthermore, the isocyanate index is 0.99-1.01, and the hard segment content is 25-30%. The catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.05-0.15%; the chain extender is polyethylene adipate, and the amount of the chain extender is 20-25% of the total mass of the polyester polyol and the diisocyanate; the end-capping agent is MPTMS, and the amount of the end-capping agent is 5-10% of the total mass of the polyester polyol and the diisocyanate.
[0045] Furthermore, the preparation step of the polyester polyol is: placing glycolide, caprolactone, 1,4-butanediol and stannous octoate in a reactor and stirring, then raising the temperature to 130-150°C for reaction for 7-9 hours, thereby obtaining the polyester polyol. The molar ratio of glycolide, caprolactone and 1,4-butanediol is 12-15:55-60:26-30, and the amount of stannous octoate is 0.5-2% of the total mass of glycolide, caprolactone and 1,4-butanediol.
[0046] Further, the diisocyanate is mixed with isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 4-6:1, wherein the preparation step of the modified isophorone diisocyanate trimer is as follows: mercaptopropyl trimethoxysilane, isophorone diisocyanate trimer and triethylamine are placed in a reactor and stirred, the temperature is raised to 70-80°C, and the reaction is carried out until the content of the isocyanate group reaches the theoretical target value to obtain the modified isophorone diisocyanate trimer. Specifically, the mass ratio of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer is 1:3-3.5, and the amount of the triethylamine is 0.01-0.05% of the total mass of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer.
[0047] Furthermore, the elastic resin compound comprises the following raw materials in parts by weight: 30-40 parts of polyurethane acrylate polymer, 15-25 parts of epoxy resin, 2-5 parts of photoinitiator, and 20-25 parts of active diluent.
[0048] Furthermore, the elastic resin compound is prepared by weighing polyurethane acrylate polymer and epoxy resin according to the formula ratio, placing them in a reactor at room temperature, and then adding a photoinitiator and a reactive diluent and mixing them thoroughly to obtain the elastic resin compound.
[0049] Furthermore, the photoinitiator is at least one of triphenyl hexafluoroantimonate, ethyl 2,4,6-trimethylbenzoylphosphonate or Irgacure 2959; the diluent is at least one of 4-vinyl cyclohexene oxide, butyl acrylate or 1,6-hexanediol diacrylate.
[0050] Furthermore, the preparation method of the polyurethane acrylate polymer comprises the following steps:
[0051] (1) placing polytetramethylene glycol, about 1 / 4 of a catalyst and a small amount of solvent in a reactor at a temperature of 60-65° C., and then slowly adding isophorone diisocyanate dropwise thereto for a reaction of 2 hours;
[0052] (2) Add about 1 / 4 of the catalyst, chain extender and a small amount of solvent into the reactor and continue the reaction for 2 hours;
[0053] (3) adding butyl 4-hydroxyacrylate and the remaining catalyst to the reactor, raising the temperature to 70-80° C., and reacting for 2-3 hours to obtain a prepolymer solution;
[0054] (4) placing the prepolymer solution obtained in step (3) at 80-90° C. to evaporate the solvent, thereby obtaining a polyurethane acrylate polymer.
[0055] Furthermore, the molar ratio of the polytetramethylene ether diol to isophorone diisocyanate is 1:3; the molar amount of the catalyst is 0.5-2% of the molar amount of the polytetramethylene ether diol; the molar ratio of the 1-hydroxybutyl acrylate to the polytetramethylene ether diol is 2:1; and the solvent is N,N-dimethylformamide.
[0056] The method for preparing the high-resilience environmentally friendly TPU shoe midsole comprises the following preparation steps:
[0057] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0058] S2, coating the front side of the thick TPU bottom layer with elastic resin rubber, and curing it with UV light to form an elastic resin layer;
[0059] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0060] Furthermore, the preparation method further comprises: in step S2, using an embossing roller to roll the elastic resin layer at a pressure of 400-600 kPa, so that the elastic resin layer is formed with a prefabricated texture structure.
[0061] Furthermore, the preparation method further comprises: in step S2, using water-based ink or bio-based ink to print different colors, patterns or texts and combinations thereof on the surface of the elastic resin layer to form a pattern layer.
[0062] Furthermore, the UV light energy density emitted by the UV machine is 800-1000mW / cm 2 .
[0063] Example 1
[0064] The present embodiment provides a high-resilience environmentally friendly TPU shoe midsole, which includes a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot-melt adhesive, and the TPU thick bottom layer is coated with an elastic resin layer on a side away from the mid-bottom layer.
[0065] Furthermore, the middle bottom layer is an EVA middle bottom layer, and the hot melt adhesive is an EVA hot melt adhesive.
[0066] Furthermore, the TPU thick bottom layer is obtained by injecting a heated molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: the polyester polyol and the diisocyanate are fully mixed, the temperature is slowly raised to 70°C, a catalyst is added to react for 4 hours, a chain extender is added thereto and the reaction is continued for 0.5 hours, the temperature is lowered to below 40°C, and then a capping agent is added thereto for capping, and the reaction is stopped after the -NCO group is completely consumed, thereby obtaining the TPU polymer.
[0067] Furthermore, the isocyanate index is 0.99, the hard segment content is 25%. The catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.05%; the chain extender is polyethylene adipate, and the amount of the chain extender is 20% of the total mass of the polyester polyol and the diisocyanate; the end-capping agent is MPTMS, and the amount of the end-capping agent is 5% of the total mass of the polyester polyol and the diisocyanate.
[0068] Furthermore, the preparation step of the polyester polyol is: placing glycolide, caprolactone, 1,4-butanediol and stannous octoate in a reactor and stirring, then raising the temperature to 130°C for reaction for 7 hours, to obtain the polyester polyol. The molar ratio of glycolide, caprolactone and 1,4-butanediol is 12:56:28, and the amount of stannous octoate is 0.5% of the total mass of glycolide, caprolactone and 1,4-butanediol.
[0069] Further, the diisocyanate is mixed with isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 4:1, wherein the preparation step of the modified isophorone diisocyanate trimer is as follows: mercaptopropyl trimethoxysilane, isophorone diisocyanate trimer and triethylamine are placed in a reactor and stirred, the temperature is raised to 70°C, and the reaction is carried out until the content of the isocyanate group reaches the theoretical target value to obtain the modified isophorone diisocyanate trimer. Specifically, the mass ratio of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer is 1:3, and the amount of the triethylamine is 0.01-0.05% of the total mass of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer.
[0070] Furthermore, the elastic resin compound comprises the following raw materials in parts by weight: 30 parts of polyurethane acrylate polymer, 15 parts of epoxy resin, 3 parts of photoinitiator, and 20 parts of active diluent.
[0071] Furthermore, the elastic resin compound is prepared by weighing polyurethane acrylate polymer and epoxy resin according to the formula ratio, placing them in a reactor at room temperature, and then adding a photoinitiator and a reactive diluent and mixing them thoroughly to obtain the elastic resin compound.
[0072] Furthermore, the photoinitiator is triphenyl hexafluoroantimonate; and the diluent is butyl acrylate.
[0073] Furthermore, the preparation method of the polyurethane acrylate polymer comprises the following steps:
[0074] (1) placing polytetramethylene glycol, about 1 / 4 of a catalyst and a small amount of solvent in a reactor at 60° C., and then slowly adding isophorone diisocyanate dropwise thereto for a reaction of 2 h;
[0075] (2) Add about 1 / 4 of the catalyst, chain extender and a small amount of solvent into the reactor and continue the reaction for 2 hours;
[0076] (3) adding butyl 4-hydroxyacrylate and the remaining catalyst to the reactor, raising the temperature to 70° C., and reacting for 2-3 hours to obtain a prepolymer solution;
[0077] (4) placing the prepolymer solution obtained in step (3) at 80° C. to evaporate the solvent, thereby obtaining a polyurethane acrylate polymer.
[0078] In the above preparation steps, the molar ratio of the polytetramethylene ether diol to isophorone diisocyanate is 1:3; the molar amount of the catalyst is 0.5% of the molar amount of the polytetramethylene ether diol; the molar ratio of the 1-hydroxybutyl acrylate to the polytetramethylene ether diol is 2:1; and the solvent is N,N-dimethylformamide.
[0079] The method for preparing the high-resilience environmentally friendly TPU shoe midsole described in this embodiment comprises the following preparation steps:
[0080] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0081] S2, apply elastic resin rubber on the front side of the thick TPU bottom layer, and cure it by UV light to form an elastic resin layer. The UV light energy density emitted by the UV machine is 800mW / cm 2 ;
[0082] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0083] Example 2
[0084] The present embodiment provides a high-resilience environmentally friendly TPU shoe midsole, which includes a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot-melt adhesive, and the TPU thick bottom layer is coated with an elastic resin layer on a side away from the mid-bottom layer.
[0085] Furthermore, the middle bottom layer is a TPU middle bottom layer, and the hot melt adhesive is a TPU hot melt adhesive.
[0086] Furthermore, the TPU thick bottom layer is obtained by injecting a heated molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: the polyester polyol and the diisocyanate are fully mixed, the temperature is slowly raised to 75°C, a catalyst is added to react for 3 hours, a chain extender is added thereto and the reaction is continued for 0.5 hours, the temperature is lowered to below 40°C, and then a capping agent is added thereto for capping, and the reaction is stopped after the -NCO group is completely consumed, thereby obtaining the TPU polymer.
[0087] Furthermore, the isocyanate index is 1.00, the hard segment content is 27%, the catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.1%, the chain extender is polyethylene adipate, and the amount of the chain extender is 22% of the total mass of the polyester polyol and the diisocyanate, and the end-capping agent is MPTMS, and the amount of the end-capping agent is 7% of the total mass of the polyester polyol and the diisocyanate.
[0088] Furthermore, the preparation step of the polyester polyol is: placing glycolide, caprolactone, 1,4-butanediol and stannous octoate in a reactor and stirring, then raising the temperature to 140°C for reaction for 8 hours, to obtain the polyester polyol. The molar ratio of glycolide, caprolactone and 1,4-butanediol is 13:58:28, and the amount of stannous octoate is 0.12% of the total mass of glycolide, caprolactone and 1,4-butanediol.
[0089] Further, the diisocyanate is a mixture of isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 5:1, wherein the preparation step of the modified isophorone diisocyanate trimer is as follows: mercaptopropyl trimethoxysilane, isophorone diisocyanate trimer and triethylamine are placed in a reactor and stirred, the temperature is raised to 75°C, and the reaction is carried out until the content of the isocyanate group reaches the theoretical target value to obtain the modified isophorone diisocyanate trimer. Specifically, the mass ratio of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer is 1:3.3, and the amount of the triethylamine is 0.03% of the total mass of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer.
[0090] Furthermore, the elastic resin compound comprises the following raw materials in parts by weight: 35 parts of polyurethane acrylate polymer, 20 parts of epoxy resin, 3 parts of photoinitiator, and 22 parts of active diluent.
[0091] Furthermore, the elastic resin compound is prepared by weighing polyurethane acrylate polymer and epoxy resin according to the formula ratio, placing them in a reactor at room temperature, and then adding a photoinitiator and a reactive diluent and mixing them thoroughly to obtain the elastic resin compound.
[0092] Furthermore, the photoinitiator is compounded from triphenyl hexafluoroantimonate and ethyl 2,4,6-trimethylbenzoylphosphonate in a mass ratio of 1:3; and the active diluent is compounded from butyl acrylate and 1,6-hexanediol diacrylate in a mass ratio of 1:2.
[0093] Furthermore, the preparation method of the polyurethane acrylate polymer comprises the following steps:
[0094] (1) placing polytetramethylene glycol, about 1 / 4 of a catalyst and a small amount of solvent in a reactor at 65° C., and then slowly adding isophorone diisocyanate dropwise thereto for a reaction of 2 h;
[0095] (2) Add about 1 / 4 of the catalyst, chain extender and a small amount of solvent into the reactor and continue the reaction for 2 hours;
[0096] (3) adding butyl 4-hydroxyacrylate and the remaining catalyst to the reactor, raising the temperature to 75° C., and reacting for 3 hours to obtain a prepolymer solution;
[0097] (4) placing the prepolymer solution obtained in step (3) at 90° C. to evaporate the solvent, thereby obtaining a polyurethane acrylate polymer.
[0098] In the above preparation steps, the molar ratio of the polytetramethylene ether diol to isophorone diisocyanate is 1:3; the molar amount of the catalyst is 1% of the molar amount of the polytetramethylene ether diol; the molar ratio of the 1-hydroxybutyl acrylate to the polytetramethylene ether diol is 2:1; and the solvent is N,N-dimethylformamide.
[0099] The method for preparing the high-resilience environmentally friendly TPU shoe midsole described in this embodiment comprises the following preparation steps:
[0100] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0101] S2, apply elastic resin rubber on the front side of the thick TPU bottom layer, and cure it by UV light to form an elastic resin layer. The UV light energy density emitted by the UV machine is 800mW / cm 2 ;
[0102] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0103] Example 3
[0104] The present embodiment provides a high-resilience environmentally friendly TPU shoe midsole, which includes a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot-melt adhesive, and the TPU thick bottom layer is coated with an elastic resin layer on a side away from the mid-bottom layer.
[0105] Furthermore, the middle bottom layer is a nylon middle bottom layer, and the hot melt adhesive is a nylon hot melt adhesive.
[0106] Furthermore, the TPU thick bottom layer is obtained by injecting a heated molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: the polyester polyol and the diisocyanate are fully mixed, the temperature is slowly raised to 80°C, a catalyst is added to react for 3 hours, a chain extender is added thereto and the reaction is continued for 1 hour, the temperature is lowered to below 40°C, and then a capping agent is added thereto for capping, and the reaction is stopped after the -NCO group is completely consumed, thereby obtaining the TPU polymer.
[0107] Furthermore, the isocyanate index is 1.01, and the hard segment content is 30%. The catalyst is dibutyltin dilaurate, and the amount of the catalyst is 0.15%; the chain extender is polyethylene adipate, and the amount of the chain extender is 25% of the total mass of the polyester polyol and the diisocyanate; the end-capping agent is MPTMS, and the amount of the end-capping agent is 10% of the total mass of the polyester polyol and the diisocyanate.
[0108] Furthermore, the preparation step of the polyester polyol is: placing glycolide, caprolactone, 1,4-butanediol and stannous octoate in a reactor and stirring, then raising the temperature to 150°C for reaction for 7 hours, to obtain the polyester polyol. The molar ratio of glycolide, caprolactone and 1,4-butanediol is 15:58:29, and the amount of stannous octoate is 2% of the total mass of glycolide, caprolactone and 1,4-butanediol.
[0109] Further, the diisocyanate is a mixture of isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 6:1, wherein the preparation step of the modified isophorone diisocyanate trimer is as follows: mercaptopropyl trimethoxysilane, isophorone diisocyanate trimer and triethylamine are placed in a reactor and stirred, the temperature is raised to 80°C, and the reaction is carried out until the content of the isocyanate group reaches the theoretical target value to obtain the modified isophorone diisocyanate trimer. Specifically, the mass ratio of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer is 1:3.5, and the amount of the triethylamine is 0.05% of the total mass of the mercaptopropyl trimethoxysilane and the isophorone diisocyanate trimer.
[0110] Furthermore, the elastic resin compound comprises the following raw materials in parts by weight: 40 parts of polyurethane acrylate polymer, 24 parts of epoxy resin, 4 parts of photoinitiator, and 22 parts of active diluent.
[0111] Furthermore, the elastic resin compound is prepared by weighing polyurethane acrylate polymer and epoxy resin according to the formula ratio, placing them in a reactor at room temperature, and then adding a photoinitiator and a reactive diluent and mixing them thoroughly to obtain the elastic resin compound.
[0112] Furthermore, the photoinitiator is Irgacure 2959; and the active diluent is 1,6-hexanediol diacrylate.
[0113] Furthermore, the preparation method of the polyurethane acrylate polymer comprises the following steps:
[0114] (1) placing polytetramethylene glycol, about 1 / 4 of a catalyst and a small amount of solvent in a reactor at 65° C., and then slowly adding isophorone diisocyanate dropwise thereto for a reaction of 2 h;
[0115] (2) Add about 1 / 4 of the catalyst, chain extender and a small amount of solvent into the reactor and continue the reaction for 2 hours;
[0116] (3) adding butyl 4-hydroxyacrylate and the remaining catalyst to the reactor, raising the temperature to 80° C., and reacting for 3 hours to obtain a prepolymer solution;
[0117] (4) placing the prepolymer solution obtained in step (3) at 90° C. to evaporate the solvent, thereby obtaining a polyurethane acrylate polymer.
[0118] In the above preparation steps, the molar ratio of the polytetramethylene ether diol to isophorone diisocyanate is 1:3; the molar amount of the catalyst is 2% of the molar amount of the polytetramethylene ether diol; the molar ratio of the 1-hydroxybutyl acrylate to the polytetramethylene ether diol is 2:1; and the solvent is N,N-dimethylformamide.
[0119] The method for preparing the high-resilience environmentally friendly TPU shoe midsole described in this embodiment comprises the following preparation steps:
[0120] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0121] S2, apply elastic resin rubber on the front side of the thick TPU bottom layer, and cure it by UV light to form an elastic resin layer. The UV light energy density emitted by the UV machine is 1000mW / cm 2 ;
[0122] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0123] Example 4
[0124] The difference between this embodiment and Embodiment 1 is: a high-rebound environmentally friendly TPU shoe midsole, the shoe midsole includes a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot-melt adhesive, the TPU thick bottom layer is coated with an elastic resin layer on a side away from the mid-bottom layer, the surface of the elastic resin layer is provided with a prefabricated texture structure, and the elastic resin layer is provided with an optical coating layer on a side away from the TPU thick bottom layer.
[0125] Furthermore, a pattern layer is provided on one side of the elastic resin layer away from the thick TPU bottom layer, and the pattern layer is formed by printing water-based ink on the surface of the elastic resin layer to form a combination of block patterns of different colors. Figure 1-2 As shown, under the action of light, the pattern layer presents discontinuously distributed white and gray block patterns, which can achieve a good anti-counterfeiting effect.
[0126] The method for preparing the high-resilience environmentally friendly TPU shoe midsole described in this embodiment comprises the following preparation steps:
[0127] S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer;
[0128] S2, coating the front side of the thick TPU bottom layer with elastic resin rubber, and curing it with UV light to form an elastic resin layer;
[0129] S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
[0130] Furthermore, the preparation method further comprises: in step S2, using an embossing roller to roll the elastic resin layer at a pressure of 500 kPa, so that the elastic resin layer is formed with a prefabricated texture structure.
[0131] Comparative Example 1
[0132] The difference between this comparative example and Example 2 is that in the step of preparing the TPU polymer, isophorone diisocyanate is used instead of the diisocyanate in Example 2.
[0133] Comparative Example 2
[0134] The difference between this comparative example and Example 2 is that in the preparation process of TPU polymer, commercially available polyester polyol (Kain Chemical, Dynacoll7360) is used to replace the polyester polyol in Example 2.
[0135] Comparative Example 3
[0136] The difference between this comparative example and Example 2 is that in the preparation of the elastic resin compound, an equal amount of epoxy resin is used to replace the polyurethane acrylate polymer, and the rest of the contents are the same as those in Example 2.
[0137] Comparative Example 4
[0138] The difference between this comparative example and Example 2 is that in the preparation of the elastic resin compound, commercially available polyurethane acrylate (Wengjiang reagent, PB072652) is used to replace the polyurethane acrylate polymer in Example 2.
[0139] The TPU midsoles prepared in the above-mentioned Examples 1-3 and Comparative Examples 1-4 are selectively tested for hardness, rebound rate, compression permanent deformation and aging resistance according to requirements, wherein the hardness adopts Shore C hardness, the rebound rate test adopts ASTM D2632-2001 standard, the compression permanent deformation adopts HG / T 4806-2015 standard, the tensile strength adopts GB / T1040.3-2006 standard, and the aging resistance is tested by QUV340nm treatment for 1000 hours at a light intensity of 800mW / cm 2 .
[0140] The test results of Examples 1-3 and Comparative Examples 1-4 are shown in Table 1 below.
[0141] Table 1 Performance test data of Examples 1-3 and Comparative Examples 1-4
[0142]
[0143] From the comparison of the above data tables, it can be seen that the TPU midsole of the present invention prepared in the above embodiments 1-3 has moderate hardness, high rebound rate and tensile strength, indicating that the TPU midsole has good rebound and shock absorption performance during use, and can improve the comfort of the sole. On the other hand, the compression permanent deformation of embodiments 1-3 is basically around 25%, indicating that it has good anti-deformation performance and long service life; and the tensile strength before and after long-term UV light exposure changes slightly, indicating that the TPU midsole has high aging resistance.
[0144] The above specific embodiments are further explanations of the technical solutions and beneficial effects of the present invention, and are not limitations of the implementation methods. For those skilled in the art, any obvious replacements that do not depart from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A high-resilience environmentally friendly TPU shoe midsole, characterized by: The shoe midsole comprises a mid-bottom layer and a TPU thick bottom layer, the mid-bottom layer and the TPU thick bottom layer are bonded by hot melt adhesive, and a side of the TPU thick bottom layer away from the mid-bottom layer is coated with an elastic resin layer; The TPU thick bottom layer is obtained by injecting a heated and molten TPU polymer into an injection molding machine for injection molding and curing, wherein the preparation steps of the TPU polymer are as follows: fully mixing polyester polyol and diisocyanate, slowly raising the temperature to 70-80°C, adding a catalyst to react for 3-4h, then adding a chain extender to continue the reaction for 0.5-1h, lowering the temperature to below 40°C, then adding a capping agent to cap the end, and stopping the reaction after the -NCO group is completely consumed, thereby obtaining the TPU polymer; The diisocyanate is prepared by mixing isophorone diisocyanate and modified isophorone diisocyanate trimer in a mass ratio of 4-6:1; The elastic resin adhesive is cured by UV light to form an elastic resin layer. The elastic resin adhesive comprises the following raw materials in parts by weight: 30-40 parts of polyurethane acrylate polymer, 15-25 parts of epoxy resin, 2-5 parts of photoinitiator, and 20-25 parts of active diluent.
2. The high-resilience environmentally friendly TPU midsole according to claim 1, characterized in that: The surface of the elastic resin layer is provided with a prefabricated texture structure, and the side of the elastic resin layer away from the TPU thick bottom layer is provided with an optical coating layer.
3. The high-resilience environmentally friendly TPU midsole according to claim 1, characterized in that: A pattern layer is provided on one side of the elastic resin layer away from the thick TPU bottom layer. The pattern layer is formed by printing water-based ink or bio-based ink on the surface of the elastic resin layer to have different colors, words or patterns and combinations thereof.
4. The high-resilience environmentally friendly TPU shoe midsole according to claim 1, characterized in that: The mid-bottom layer is any one of an EVA mid-bottom layer, a TPU mid-bottom layer or a nylon mid-bottom layer.
5. The high-resilience environmentally friendly TPU shoe midsole according to claim 1, characterized in that: The hot melt adhesive is any one of EVA hot melt adhesive, TPU hot melt adhesive or nylon hot melt adhesive.
6. The high-resilience environmentally friendly TPU shoe midsole according to claim 1, characterized in that: In the preparation step of the TPU polymer, the isocyanate index is 0.99-1.01, the hard segment content is 25-30%, and the amount of the chain extender is 20-25% of the total mass of the polyester polyol and the diisocyanate.
7. The high-resilience environmentally friendly TPU shoe midsole according to claim 1, characterized in that: Glycolide, caprolactone, 1,4-butanediol and stannous octoate are placed in a reactor and stirred, and then the temperature is raised to 130-150° C. for reaction for 7-9 hours to obtain the polyester polyol; wherein the molar ratio of glycolide, caprolactone and 1,4-butanediol is 12-15:55-60:26-30.
8. The method for preparing the high-resilience environmentally friendly TPU shoe midsole according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: S1. Use an injection molding machine to mold a TPU thick bottom layer, and stick a PET film on the back of the TPU thick bottom layer; S2, coating the front side of the thick TPU bottom layer with elastic resin rubber, and curing it with UV light to form an elastic resin layer; S3, cutting the obtained TPU thick bottom layer according to the size requirements, removing the PET film on the back of the cut TPU thick bottom layer, then applying hot melt adhesive, and pressing it together with the middle bottom layer to obtain the TPU shoe midsole.
Citation Information
Patent Citations
Low-density high-strength high-yellowing-resistant TPU for soles, and preparation method thereof
CN110627983A
Method for preparing polyester polyol from glycolide-epsilon-caprolactone copolymer
CN113667101A
Two-dimensional (2D) colorful wear-resistant non-slip shoe outsole
CN216165563U
Basketball shoes with foot protecting and bouncing assisting functions
CN220192316U