A die-cast aluminum alloy material and its preparation method, and automotive structural components.
By optimizing the element ratio and alloying control of die-cast aluminum alloy materials, heat-free die-cast aluminum alloy materials were prepared, solving the problem of mechanical property changes of electric drive systems under high temperature conditions, and achieving improvements in high strength, creep resistance, and cost reduction.
Patent Information
- Application Number
- CN202410330702.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Existing die-cast aluminum alloy materials exhibit significant changes in mechanical properties when used under high-temperature conditions, failing to meet the requirements of electric drive systems for high strength and creep resistance. Furthermore, conventional testing methods cannot reflect the performance of components under actual operating conditions.
By optimizing the elemental composition of die-cast aluminum alloy materials, including the contents of Si, Mn, Cu, Mg, Zn, Ti, Sr, Zr, Ni, and Bi, and combining alloying control and grain refinement strengthening, heat-free die-cast aluminum alloy materials suitable for motor housings are prepared.
It achieves improved strength, tensile strength and elongation of die-cast aluminum alloy materials under high temperature conditions, improves high temperature performance and creep resistance, reduces costs and carbon emissions, and is suitable for the chassis environment of electric drive systems.
Smart Images

Figure CN118028667B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to the field of die-cast aluminum alloy technology, specifically to a die-cast aluminum alloy material and its preparation method, and automotive structural components. Background Technology
[0002] Aluminum alloys are widely used in die-cast housings of motors due to their advantages such as low density, good thermal conductivity, and good flow properties. Currently, the most widely used die-cast aluminum alloy material in industry is the AlSiCu series alloy.
[0003] Similarly, with the development of new energy vehicles, the electric drive industry is constantly pursuing the ultimate power density, resulting in extreme requirements for lightweighting and high power. This has led to the development of electric drive housings using high-strength die-cast aluminum alloys. High-strength, high-yield electric drive housings can simultaneously address the requirements of lightweighting and high power. The high strength allows for localized thinning designs, resulting in weight reduction benefits, while also meeting the strength requirements of high power and high torque. In some of the highest-performance electric drives, the yield strength of the electric drive housing itself is even required to reach over 240 MPa. Therefore, the development of ultra-high-strength, heat-free aluminum alloys for electric drive housings is imperative.
[0004] Furthermore, the performance of conventional aluminum alloys is tested on die-cast or cast test bars or pieces, which differs significantly from the performance tested on actual components, and there is no clear correlation. Therefore, to more accurately reflect the material's performance in actual parts, greater attention should be paid to the intrinsic performance of the electric drive housing, i.e., sampling and testing on the component itself. Simultaneously, the operating temperature of motors can reach up to 120℃, and may even be higher in some designs; therefore, while considering the material's room temperature performance, meeting high-temperature performance requirements is also essential. Regarding the mechanical properties of metals, the commonly used testing method is a uniaxial tensile test at room temperature to obtain the stress-strain curve. However, in fields such as energy, chemical engineering, metallurgy, and aerospace, many components must operate under high-temperature conditions for extended periods. For example, the operating parameters of ultra-supercritical thermal power units in power plants can reach 26.25 MPa and 600℃. For metallic materials used under high-temperature conditions, using only the mechanical properties under short-term static load at room temperature as the basis for material selection is clearly insufficient, because the mechanical properties of materials change significantly under high-temperature service environments. Even when the working stress is less than the yield strength of the material at the working temperature, the material will still undergo slow and continuous plastic deformation (i.e., creep) during long-term service. Therefore, in order to prevent the motor from creeping failure during long-term operation, it is necessary to further investigate the creep resistance of the material. Summary of the Invention
[0005] The purpose of this disclosure is to provide a die-cast aluminum alloy material and its preparation method, as well as automotive structural parts, which can improve the yield strength, tensile strength and elongation of the die-cast material under heat treatment-free conditions to meet the body performance requirements of electric drive housings; it can also improve the high-temperature performance and creep resistance of the die-cast material.
[0006] To achieve the above objectives, the first aspect of this disclosure provides a die-cast aluminum alloy material, wherein, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: 8.5 to 13 wt% Si, 0.1 to 1 wt% Mn, 0 to 0.5 wt% Fe, 1.5 to 3 wt% Cu, 0.5 to 2 wt% Mg, 1.0 to 2.5 wt% Zn, 0.02 to 0.5 wt% Ti, 0.02 to 0.08 wt% Sr, 0.02 to 0.1 wt% Zr, 0 to 0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al.
[0007] Optionally, the die-cast aluminum alloy material further contains Bi; preferably, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material includes 0.01~0.1% by weight of Bi.
[0008] Optionally, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: 8.8~12 wt% Si, 0.2~0.8 wt% Mn, 0~0.5 wt% Fe, 1.5~3.0 wt% Cu, 0.03~0.1 wt% Bi, 0.5~2.0 wt% Mg, 1.3~2.3 wt% Zn, 0.02~0.5 wt% Ti, 0.02~0.08 wt% Sr, 0.02~0.1 wt% Zr, 0~0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al.
[0009] Optionally, in the die-cast aluminum alloy material, the ratio of Cu to Bi content is less than 40, and optionally, the ratio of Cu to Ni content is less than 50.
[0010] Optionally, the die-cast aluminum alloy material does not contain Mo.
[0011] Optionally, the intrinsic properties of the die-cast aluminum alloy material include: a yield strength of 240 MPa or more, a tensile strength of 320 MPa or more, and an elongation of 1.5% or more.
[0012] A second aspect of this disclosure provides a method for preparing die-cast aluminum alloy materials, comprising the following steps: S1. The alloy raw material mixture is smelted in a smelting furnace to obtain a first alloy melt. The alloy raw material mixture includes: 8.5~13 wt% Si, 0.1~1 wt% Mn, 0~0.5 wt% Fe, 1.5~3 wt% Cu, 0.5~2 wt% Mg, 1.0~2.5 wt% Zn, 0.02~0.5 wt% Ti, 0.02~0.08 wt% Sr, 0.02~0.1 wt% Zr, 0~0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al. S2. The first alloy melt is subjected to degassing, refining and first slag removal in a converter to obtain the second alloy melt. S3. The second alloy melt is subjected to heat preservation treatment and second slag removal treatment in a machine-side furnace to obtain the third alloy melt. S4. The third alloy melt is subjected to die casting treatment.
[0013] Optionally, in step S1, the conditions for the smelting process include: a smelting temperature of 740~760℃, a smelting atmosphere temperature of 700~950℃, and a smelting time of 3~13h.
[0014] Optionally, in step S2, the conditions for degassing include: a degassing speed of 400~500 r / min, a degassing gas source pressure of 0.35~0.45 MPa, a degassing temperature of 760~770℃, and a degassing time of 8~10 min; The refining process includes: introducing nitrogen gas containing refining agent powder into the first melt after degassing for a first refining, and then introducing nitrogen gas containing refining agent powder again for a second refining. The first slag removal process includes removing slag using slag removal tools.
[0015] Optionally, in step S3, the conditions for the heat preservation treatment include: heat preservation temperature of 660~680℃ and heat preservation time of 30~40min; The second slag removal process includes removing slag using slag removal tools.
[0016] Optionally, in step S4, the conditions for the die casting process include: casting pressure above 60 MPa, high speed above 3.5 m / s, vacuum degree below 100 mbar, aluminum liquid temperature above 660~680℃, mold coating temperature above 120~150℃, and injection delay time below 1 s.
[0017] This disclosure provides a third aspect of providing die-cast aluminum alloy materials prepared according to the method described in the second aspect of this disclosure.
[0018] The fourth aspect of this disclosure provides an automotive structural component, including a die-cast aluminum alloy material, wherein the die-cast aluminum alloy material is the heat-free die-cast aluminum alloy material described in the first or third aspect of this disclosure.
[0019] Through the above technical solutions, this disclosure provides a die-cast aluminum alloy material and its preparation method, as well as automotive structural parts. This aluminum alloy material, through alloying control and AI model iteration, explores the elemental ratios and contents of the alloy material to achieve composite modification and fine-grain strengthening effects, resulting in a material with optimal strength and elongation suitable for motor housings. The performance of the die-cast aluminum alloy disclosed herein has been fully verified on motor housing molds. On the motor cylinder wall (i.e., the location where the motor requires the highest strength), body sampling performance can be achieved, and the die-cast aluminum alloy material exhibits high strength and elongation; and Cu... With a lower content, it has better corrosion resistance from an alloying perspective; furthermore, the high-temperature performance and creep resistance of the die-cast aluminum alloy material disclosed herein are also improved, making it suitable for electric drive applications located in the chassis; the die-cast aluminum alloy of this disclosure can achieve the performance of other conventional alloys after heat treatment without heat treatment, which saves costs and reduces carbon emissions, and also provides significant benefits for the dimensional accuracy of parts; the die-cast aluminum alloy of this disclosure has a lower cost, does not contain rare earth elements, and has relatively lower iron content requirements compared to other high-strength aluminum alloys, which is conducive to the use of recycled materials, further reducing costs.
[0020] Other features and advantages of this disclosure will be described in detail in the following detailed description section. Attached Figure Description
[0021] The accompanying drawings are provided to further illustrate the present disclosure and form part of the specification. They are used together with the following detailed description to explain the present disclosure, but do not constitute a limitation thereof. In the drawings: Figure 1 A schematic flowchart of the method for preparing die-cast aluminum alloy materials according to this disclosure is shown; Figure 2 The diagram shows the motor housing and sampling location of the die-cast aluminum alloy used for body sampling.
[0022] Explanation of reference numerals in the attached figures 1-Sampling location of the body. Detailed Implementation
[0023] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.
[0024] The first aspect of this disclosure provides a die-cast aluminum alloy material, wherein, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: 8.5 to 13 wt% Si (silicon), 0.1 to 1 wt% Mn (manganese), 0 to 0.5 wt% Fe (iron), 1.5 to 3 wt% Cu (copper), 0.5 to 2 wt% Mg (magnesium), 1.0 to 2.5 wt% Zn (zinc), 0.02 to 0.5 wt% Ti (titanium), 0.02 to 0.08 wt% Sr (strontium), 0.02 to 0.1 wt% Zr (zirconium), 0 to 0.1 wt% Ni (nickel), less than 0.1 wt% impurities, and the balance being Al (aluminum).
[0025] This disclosure provides a die-cast aluminum alloy material. Through alloying control and AI model iteration, the material achieves composite modification and fine-grain strengthening effects by exploring the proportions of alloying elements such as Cu, Mg, Ni, Zr, and Zn. This results in a material with optimal strength and elongation suitable for motor housings. The performance of the die-cast aluminum alloy disclosed herein has been fully verified on motor housing molds. Sampling performance can be achieved at the motor cylinder wall (the location requiring the highest strength). The die-cast aluminum alloy material exhibits high strength and elongation, and its lower Cu content results in better corrosion resistance from an alloying perspective. Furthermore, the high-temperature performance and creep resistance of the die-cast aluminum alloy disclosed herein are also improved, making it suitable for electric drive applications located in the chassis. The die-cast aluminum alloy of this disclosure achieves the performance of other conventional alloys after heat treatment without requiring heat treatment. Eliminating heat treatment saves costs and reduces carbon emissions, while also significantly improving the dimensional accuracy of components. The die-cast aluminum alloy of this disclosure has a lower cost, does not contain rare earth elements, and has lower iron content requirements compared to other high-strength aluminum alloys, facilitating the use of recycled materials and further reducing costs.
[0026] In this disclosure, impurities may include Cr (chromium), Sn (tin), Pb (lead), etc. The total amount of impurities in the die-cast aluminum alloy material provided in this disclosure is less than 0.1% by weight.
[0027] In a preferred embodiment, the die-cast aluminum alloy material further contains Bi (bismuth) element; preferably, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material includes 0.01~0.1% by weight of Bi.
[0028] In a preferred embodiment, the die-cast aluminum alloy material does not contain Mo (molybdenum). The inventors of this disclosure have discovered several technical challenges in adding molybdenum powder: firstly, the amount of molybdenum powder added must be precise; excessive molybdenum powder can cause the aluminum alloy to become brittle; secondly, the uniformity of molybdenum powder distribution is crucial to the performance of the aluminum alloy; uneven distribution can lead to a reduction in the strength and toughness of the aluminum alloy material. The die-cast aluminum alloy material provided by this disclosure does not contain the metallic element Mo, thus avoiding the aforementioned drawbacks caused by metallic Mo and contributing to cost reduction.
[0029] Silicon is the main element in most aluminum alloys. It improves the fluidity of the alloy at high temperatures and increases its tensile strength, but it reduces its plasticity. When the silicon content in an alloy exceeds the eutectic composition, and there are also many impurities such as copper and iron, free silicon is generated. Free silicon has a very high hardness, causing severe tool wear during machining. In addition, in high-silicon aluminum alloys, silicon usually exists in the aluminum alloy as a coarse acicular structure, which reduces the mechanical properties of the alloy. Through research and exploration, the inventors of this disclosure have found that the optimal range for controlling the Si content in die-cast aluminum alloy materials is 8.5~13% by weight, which can meet the elongation requirements of motor housings, provide impact resistance, and also improve the strength of the alloy material to a high level.
[0030] Iron: The higher the iron content, the better the recyclability of the material and the better the demolding effect. However, excessive iron content will produce brittle needle-like phases, which is detrimental to performance. This disclosure controls the upper limit of Fe content in die-cast aluminum alloy materials to 0.5% by weight, which can ensure excellent material performance while achieving high demolding and recycling effects.
[0031] Copper: Copper is an important alloying element with a certain solid solution strengthening effect. In addition, CuAl2 precipitated during aging has a significant age-hardening effect. The inventors of this disclosure have found that controlling the copper content in die-cast aluminum alloys between 1.5% and 3.0% by weight can improve the age-hardening effect of the alloy while maintaining the corrosion resistance of the alloy material, which is superior to conventional alloys such as A380 and ADC12.
[0032] Bismuth: The addition of Cu will form a strengthening phase CuAl2, but the morphology of CuAl2 also has a great influence on performance. After a lot of experiments and research, the inventors of this disclosure have found that adding a certain amount of bismuth (0.01~0.10 wt%) can make the α-Al / CuAl2 binary eutectic in the alloy material gradually change from a coarse radial shape to a uniform and fine short lamellar structure, and the long needle-like morphology of eutectic silicon changes to a dot needle shape, which is beneficial to improving the strength, high temperature performance and creep resistance of the material.
[0033] Magnesium: Adding a small amount of magnesium to high-silicon aluminum alloys can improve the alloy's tensile strength, elastic limit, fatigue limit, and hardness; however, the presence of magnesium increases the alloy's oxidation tendency during melting and heat treatment. Magnesium is a significant strength-enhancing element. The combined addition of Mg and Cu, in addition to the CuAl2 and Mg2Si phases, also results in complex strengthening phases such as Q-Al5Mg8Si6Cu2. After multiple second-phase combinations, the alloy's heat resistance temperature can reach 250℃. The inventors of this disclosure have focused on magnesium content, controlling it to 0.5~2% by weight. This allows for control of the elongation of the die-cast aluminum alloy material to meet the basic requirements of motor housings, while also effectively improving strength and avoiding the drawback of low elongation caused by excessive magnesium content.
[0034] Zinc: It has good casting and mechanical properties. The zinc content is controlled at 1.0~2.5% by weight in this disclosure, which can avoid the adverse effects of zinc on the alloy's tendency to hot crack and the reduction of corrosion resistance. Titanium: As an effective nucleating agent in aluminum alloys, the present disclosure controls the titanium content in the range of 0.02~0.5% by weight, which can significantly refine the grain size of aluminum alloys and improve room temperature mechanical properties and rolling properties of aluminum alloys; at the same time, the formed Al3Ti phase has the characteristics of high melting point and high hardness, and can also improve the high temperature strength of aluminum alloys.
[0035] Strontium is an effective spheroidizing agent for eutectic silicon. The present disclosure adds 0.02 to 0.08% by weight of Sr, which can transform eutectic silicon from needle-like to fibrous, thus helping to improve the strength and toughness of die-casting materials.
[0036] Zirconium: It readily forms (Al,Si)3Zr particles in alloys, which can easily become heterogeneous nucleation sites for α-Al, refining the grains and simultaneously improving the strength and elongation of the alloy. The die-cast aluminum alloy material disclosed herein includes 0.02~0.1% by weight of zirconium, which can avoid the adverse effects on alloy properties caused by the coarsening of (Al,Si)3Zr particles and high Zr content, while also leveraging the beneficial effects of the thermally stable Al3Zr phase on the high-temperature properties of aluminum alloy materials.
[0037] Manganese: Manganese can transform the lamellar or needle-like crystal structure of iron in aluminum alloys into a fine crystal shape. The presence of manganese can reduce the harmful effects of iron. This disclosure adds 0.1 to 1% by weight of Mn to aluminum alloy materials, which can reduce the problem of poor demolding caused by low iron content in aluminum alloys, and at the same time avoid the segregation phenomenon caused by high manganese content in the alloy.
[0038] Nickel: Adding an appropriate amount of Ni (0~0.1% by weight) to the aluminum alloy material disclosed herein can improve the high-temperature mechanical properties of the aluminum alloy, and the Al7Cu4Ni intermetallic compound formed can also increase the stability of the microstructure at high temperature.
[0039] In a preferred embodiment, based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: The composition of the die-cast aluminum alloy material provided in this embodiment is 8.8–12 wt% Si, 0.2–0.8 wt% Mn, 0–0.5 wt% Fe, 1.5–3.0 wt% Cu, 0.03–0.1 wt% Bi, 0.5–2.0 wt% Mg, 1.3–2.3 wt% Zn, 0.02–0.5 wt% Ti, 0.02–0.08 wt% Sr, 0.02–0.1 wt% Zr, 0–0.1 wt% Ni, and less than 0.1 wt% impurities with the balance being Al. This embodiment provides a composition ratio that is beneficial for further improving the performance of the aluminum alloy material.
[0040] In a preferred embodiment, the ratio of Cu to Bi in the die-cast aluminum alloy material is 40 or less, and optionally, the ratio of Cu to Ni is 50 or less. The inventors of this disclosure have discovered that when the ratios of Cu to Bi and Cu to Ni in the die-cast aluminum alloy are within the optimized ranges provided in this embodiment, the die-cast aluminum alloy material can possess superior strength properties, high-temperature properties, and creep resistance.
[0041] In one specific embodiment, the bulk properties of the die-cast aluminum alloy material include (at room temperature): a yield strength of ≥240 MPa, a tensile strength of ≥320 MPa, and an elongation of ≥1.5%; preferably, the yield strength is ≥250 MPa, the tensile strength is ≥330 MPa, and the elongation is ≥3%. The bulk properties of the die-cast aluminum alloy material provided in this disclosure can meet the target of extreme power torque in electric drives.
[0042] In this disclosure, the bulk properties of die-cast aluminum alloy materials refer to the strength properties of the bulk material obtained by taking a tensile specimen that meets the requirements from a part used in actual application and conducting a tensile test. The bulk material can be sampled using the following method: first, the bulk material of the part is obtained through a die-casting process; the area that meets the requirements for a tensile specimen is marked; then, the marked sample block is obtained by cutting; and a standard tensile specimen is obtained from the sample block using a wire EDM method.
[0043] In one specific embodiment, the yield strength of the flat mold sample of the aluminum alloy die-casting material at 120°C is above 250 MPa, the tensile strength is above 320 MPa, and the elongation is above 2%. Conventional ADC12 aluminum alloy materials, tested under the same conditions, have a yield strength above 180 MPa, a tensile strength above 270 MPa, and an elongation above 2%. A horizontal comparison between the aluminum alloy of this disclosure and existing ADC12 aluminum alloys shows that the die-casting aluminum alloy material provided in this disclosure has better high-temperature performance.
[0044] In one specific embodiment, the total strain of the die-cast flat mold sample of the aluminum alloy die-casting material is 0.155%. Under the same conditions, the total strain of ADC12 is 0.200%. Through a lateral comparison of the two materials, it can be seen that the die-cast aluminum alloy material provided in this disclosure has better creep resistance.
[0045] A second aspect of this disclosure provides a method for preparing die-cast aluminum alloy materials, comprising the following steps: S1. The alloy raw material mixture is smelted in a smelting furnace to obtain a first alloy melt. The alloy raw material mixture includes: 8.5~13 wt% Si, 0.1~1 wt% Mn, 0~0.5 wt% Fe, 1.5~3 wt% Cu, 0.5~2 wt% Mg, 1.0~2.5 wt% Zn, 0.02~0.5 wt% Ti, 0.02~0.08 wt% Sr, 0.02~0.1 wt% Zr, 0~0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al. S2. The first alloy melt is subjected to degassing, refining and first slag removal in a converter to obtain the second alloy melt. S3. The second alloy melt is subjected to heat preservation treatment and second slag removal treatment in a machine-side furnace to obtain the third alloy melt. S4. The third alloy melt is subjected to die casting treatment.
[0046] The method for preparing die-cast aluminum alloys disclosed herein can obtain high-strength aluminum alloy materials without heat treatment, thus avoiding the drawbacks of reduced production efficiency, increased production costs, and additional carbon emissions that would result from heat treatment.
[0047] This disclosure describes the preparation of alloy ingots using smelting equipment (including smelting furnaces, converters, machine-side furnaces, etc.) to melt the ingots (or perform furnace cleaning operations, subject to passing composition testing). The smelting equipment is a conventional device structure in this field.
[0048] In a preferred embodiment, the alloy raw material mixture comprises: The alloy comprises 8.8–12 wt% Si, 0.2–0.8 wt% Mn, 0–0.5 wt% Fe, 1.5–3.0 wt% Cu, 0.03–0.1 wt% Bi, 0.5–2.0 wt% Mg, 1.3–2.3 wt% Zn, 0.02–0.5 wt% Ti, 0.02–0.08 wt% Sr, 0.02–0.1 wt% Zr, 0–0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al. The die-cast aluminum alloy prepared according to the optimized alloy raw materials provided in this embodiment exhibits better strength and elongation properties, and its high-temperature performance and creep resistance are further improved.
[0049] In one embodiment, in step S1, the conditions for the smelting process include: a smelting temperature of 740~760℃, a smelting atmosphere temperature of 700~950℃, and a smelting time of 3~13h; preferably, the smelting temperature is 745~755℃, the smelting atmosphere temperature is 750~850℃, and the smelting time is 5~8h.
[0050] In one embodiment, in step S2, the degassing conditions include: a degassing speed of 400-500 r / min, a degassing gas source pressure of 0.35-0.45 MPa, a degassing temperature of 760-770°C, and a degassing time of 8-10 min; preferably, the degassing speed is 450-500 r / min, the degassing gas source pressure is 0.4-0.45 MPa, the degassing temperature is 765-770°C, and the degassing time is 9-10 min. The refining process includes: introducing nitrogen gas containing refining agent powder into the first melt after degassing for a first refining process, and introducing nitrogen gas containing refining agent powder again for a second refining process; wherein the refining agent is a type conventionally selected in the art and can be obtained through ordinary commercial channels; The first slag removal process includes removing slag using slag removal tools.
[0051] In one embodiment, in step S3, the conditions for the heat preservation treatment include: a heat preservation temperature of 660~680℃ and a heat preservation time of 30~40min; preferably, the heat preservation temperature is 670~680℃ and the heat preservation time is 35~40min. The second slag removal process includes removing slag using slag removal tools.
[0052] In one embodiment, in step S4, the die-casting equipment is a Lijing DC2500 die-casting machine, and the die-casting conditions include: casting pressure above 60 MPa, high-speed speed above 3.5 m / s, vacuum degree below 100 mbar, aluminum liquid temperature of 660~680℃, mold temperature after spraying above 120~150℃, and injection delay time below 1 s. Preferably, the casting pressure is 80~100 MPa, high-speed speed above 4.5 m / s, vacuum degree of 50~60 mbar, aluminum liquid temperature of 670~680℃, mold temperature after spraying above 140~150℃, and injection delay time below 1 s.
[0053] In one embodiment, the method further includes: performing a first component detection process on the first alloy melt obtained in step S1; and when the result of the first component detection process meets a first condition, causing the first alloy melt to proceed to step S2. The second alloy melt obtained in step S2 is subjected to a second composition detection process; when the result of the second composition detection process meets the second condition, the second alloy melt is subjected to step S3. The third alloy melt obtained in step S3 is subjected to a third component detection process; when the result of the third component detection process meets the third condition, the third alloy melt is subjected to step S4. Optionally, the first condition, the second condition, and the third condition each independently include: The alloy melt composition includes: 8.5-13 wt% Si, 0.1-1 wt% Mn, 0-0.5 wt% Fe, 1.5-3 wt% Cu, 0.5-2 wt% Mg, 1.0-2.5 wt% Zn, 0.02-0.5 wt% Ti, 0.02-0.08 wt% Sr, 0.02-0.1 wt% Zr, 0-0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al; preferably 8.8- The alloy composition comprises 12 wt% Si, 0.2–0.8 wt% Mn, 0–0.5 wt% Fe, 1.5–3.0 wt% Cu, 0.03–0.1 wt% Bi, 0.5–2.0 wt% Mg, 1.3–2.3 wt% Zn, 0.02–0.5 wt% Ti, 0.02–0.08 wt% Sr, 0.02–0.1 wt% Zr, 0–0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al. In this disclosure, the composition of the alloy melt obtained at each step of the preparation process is analyzed to ensure that the final alloy material meets the required composition.
[0054] The third aspect of this disclosure provides cast aluminum alloy materials prepared according to the method described in the second aspect of this disclosure.
[0055] The fourth aspect of this disclosure provides an automotive structural component, including a die-cast aluminum alloy material, wherein the die-cast aluminum alloy material is the heat-free die-cast aluminum alloy material described in the first or third aspect of this disclosure.
[0056] Furthermore, the automotive structural components include parts formed by die casting that require high strength and high yield strength, including but not limited to electric drive components such as motor housings, motor end covers, and reducer housings. Figure 2 As shown, Figure 2 The structure shown is a motor housing, wherein the main body sampling position 1 is on the motor housing.
[0057] The present invention will be further described in detail below through examples. All raw materials used in the examples are commercially available.
[0058] Example 1 This embodiment describes the preparation of aluminum alloy materials according to the alloy raw material composition listed in Table 1, and the conditions include: (1) Place the prepared alloy ingot into the melting furnace, set the melting temperature to 750℃, the melting atmosphere temperature to 850℃, and the melting time to 8h, fully melt it, and test whether its composition meets the requirements (by taking a small part of the melt and solidifying it, and then performing OES (Optical Emission Spectroscopy) composition detection method). After passing the test, proceed to the next step. (2) The molten alloy solution is transferred to a converter for degassing, refining and slag removal. The degassing conditions are as follows: degassing speed is 450 r / min, degassing gas source pressure is 0.4 MPa, temperature is 765℃ and time is 10 min. The refining conditions are as follows: at a temperature of 760℃, a refining agent is added for the first refining, and nitrogen gas containing refining agent powder is introduced for the second refining. During the refining process, the mixture is stirred evenly and gently, and then left to stand for 10 minutes. Then, the slag is skimmed off using a slag removal tool. The composition is checked to see if it meets the requirements. If it is qualified, the next step is carried out. (3) Transfer the alloy solution from the transfer furnace to the machine side furnace for heat preservation and slag removal. The heat preservation temperature is 680℃ and the heat preservation time is 30 minutes. Check whether its composition meets the requirements. After passing the test, proceed to the next step. S4: Die casting is performed. The die casting parameters include: press tonnage of 2500 Ton, casting pressure of 60 MPa or above, high speed of 3.5 m / s, vacuum degree of 60 mbar, aluminum liquid temperature of 660℃, mold coating temperature of 150℃, and injection delay time of 1 s.
[0059] Examples 2-7 Examples 2-7 follow the preparation method in Example 1, except that the aluminum alloy materials are prepared according to the alloy raw material composition listed in Table 1, and the rest of the process is the same as in Example 1.
[0060] Example 8 This embodiment prepares the alloy raw material mixture according to the raw material formula in Example 1, but differs from Example 1 in that the preparation process conditions are changed: (1) Place the prepared alloy ingot into the melting furnace, set the melting temperature to 790℃, the melting atmosphere temperature to 850℃, and the melting time to 10h, fully melt it, and check whether its composition meets the requirements. After it is qualified, proceed to the next step. (2) Transfer the molten alloy solution to a converter for degassing, refining, and slag removal. The degassing conditions include: a degassing speed of 380 r / min, a degassing gas source pressure of 0.3 MPa, a temperature of 780℃, and a time of 3 min. The refining conditions include: adding a refining agent at a temperature of 780℃ for the first refining treatment, then introducing nitrogen gas containing refining agent powder for the second refining treatment, while simultaneously stirring gently and evenly, letting it stand for 3 minutes, and then using a slag removal tool to skim off the slag. Check whether its composition meets the requirements. If it is qualified, proceed to the next step. (3) Transfer the alloy solution from the transfer furnace to the machine side furnace for heat preservation and slag removal. The heat preservation temperature is 680℃ and the heat preservation time is 1h. Check whether its composition meets the requirements. If it meets the requirements, proceed to the next step. S4: Die casting is performed. The die casting parameters include: press tonnage of 3000 Ton, casting pressure of 60 MPa or above, high speed of 3 m / s, vacuum degree of 100 mbar, aluminum liquid temperature of 680℃, mold temperature after spraying of 150℃, and injection delay time of 1 s.
[0061] Comparative Examples 1-9 Comparative Examples 1-9 were prepared according to the preparation method in Example 1, except that the aluminum alloy materials were prepared according to the alloy raw material composition listed in Table 1, and the rest of the process was the same as in Example 1.
[0062] Comparative Example 10 This comparative example uses the formula and preparation process described in Example 1 of CN116752018A to prepare aluminum alloy materials.
[0063] Table 1
[0064] In the alloy formula, "-" indicates that it is not added or does not exist; in the Cu / Bi and Cu / Ni content ratio data, "-" indicates that the calculation result cannot be obtained because the Bi or Ni content is 0 (or the result can be considered as infinity).
[0065] Test Example 1 This test example is used to sample the products prepared in the above embodiments and comparative examples and to test their mechanical properties.
[0066] The method for sampling the body is as follows: First, the body of the part is obtained through die casting. The area that meets the requirements for tensile test specimens is marked. Then, the marked sample blocks are obtained by cutting. Standard tensile test specimens are obtained from the sample blocks by wire cutting with slow wire cutting. The sample specifications are according to the small size test of ASTM E8. The thickness is the actual thickness of the body, about 5~6mm. Tensile test specimens are taken.
[0067] The test methods for yield strength, tensile strength and elongation of the specimens were in accordance with standard GB / T 228.1-2021 Metallic materials, tensile testing—Part 1: Tests at room temperature. The test results are listed in Table 2 below.
[0068] Table 2
[0069] According to the data in Table 2 above: Comparing Examples 1-7 with Comparative Examples 1-10, it can be seen that the metal ratios provided in this disclosure were not used in the alloy preparation in Comparative Examples 1-10. The heat-free die-cast aluminum alloy materials obtained in Examples 1-7 have higher yield strength and tensile strength while ensuring higher elongation, and have better overall performance.
[0070] Comparing Examples 1-2 with Examples 3-7, it can be seen that the alloy composition of Examples 1-2 is within the preferred range provided in this disclosure. Compared with Examples 3-7, the aluminum alloy materials obtained by Examples 1-2 have higher yield strength, tensile strength and elongation.
[0071] Comparing Example 3 and Example 4, the aluminum alloy material of Example 4 did not contain metallic Bi, while the aluminum alloy material of Example 3 contained metallic Bi. The strength properties of the aluminum alloy material obtained in Example 3 were better than those in Example 4. Comparing Example 3 with Example 2, it can be seen that the alloy composition of Example 2 is within the preferred range provided in this disclosure, and the mass ratio of Cu to Bi is not higher than 40. Compared with Example 3, Example 2 has better strength properties and elongation. Comparing Example 2 with Example 1, it can be seen that the alloy composition of Example 1 is within the preferred range provided in this disclosure, and the mass ratio of Cu to Ni in Example 1 is not higher than 50. The yield strength and tensile strength of the aluminum alloy material obtained in Example 1 are significantly improved compared with the aluminum alloy material in Example 2. Comparing Example 1 with Example 8, it can be seen that the aluminum alloy material prepared in Example 1 according to the optimized process conditions provided in this disclosure has higher yield strength, tensile strength and elongation.
[0072] Test Example 2 This test example is used to test the high-temperature performance of aluminum alloy materials prepared in Examples 1-7, Comparative Example 1 (ADC12 alloy), and Comparative Example 10.
[0073] The test method for mechanical properties of the test bar at 120℃ includes: referring to GB / T 228.2-2015 "Metallic materials, tensile testing - Part 2: High temperature test method", using the Landmark 370.25 electro-hydraulic servo fatigue testing machine.
[0074] The test results are listed in Table 3 below.
[0075] Table 3
[0076] According to the data in Table 3 above: Compared with Comparative Examples 1 and 10, the alloy materials obtained in Examples 1 to 7, under the test condition of 120°C, have higher yield strength and tensile strength while ensuring higher elongation. That is, the aluminum alloy materials obtained in Examples 1 to 7 according to the method provided in this disclosure have better high-temperature performance. Comparing Examples 1-2 with Examples 3-7, it can be seen that the alloy composition of Examples 1-2 is within the preferred range provided in this disclosure. Compared with Examples 3-7, the aluminum alloy materials obtained by Examples 1-2 have better high-temperature performance and can simultaneously take into account strength performance and elongation. Comparing Example 3 and Example 4, the aluminum alloy material in Example 4 did not contain metallic Bi, while the aluminum alloy material in Example 3 contained metallic Bi. The high-temperature performance of the aluminum alloy material obtained in Example 3 was better than that in Example 4. Comparing Example 3 with Example 2, it can be seen that the alloy composition of Example 2 is within the preferred range provided in this disclosure, and the mass ratio of Cu to Bi is not higher than 40. Compared with Example 3, Example 2 has better high-temperature performance. Comparing Example 2 with Example 1, it can be seen that the alloy composition of Example 1 is within the preferred range provided in this disclosure, and the mass ratio of Cu to Ni in Example 1 is not higher than 50. The high-temperature performance of the aluminum alloy material obtained in Example 1 is significantly better than that of the aluminum alloy material in Example 2.
[0077] Test Example 3 This test example is used to test the anti-creep performance of the aluminum alloy materials prepared by Example 1 and Comparative Example 1 (ADC12 alloy) and 10.
[0078] The method for testing the creep resistance of a flat plate mold includes: referring to GB / T2039 "Metallic Materials - Uniaxial Tensile Creep Test Method", the test temperature is 120℃, the initial load is 90MPa, the creep time is 100h, and the equipment is a creep testing machine RDL-10.
[0079] The test results are listed in Table 4 below.
[0080] Table 4
[0081] As can be seen from the data in Table 4 above, compared with Comparative Examples 1 and 10, the aluminum alloy material provided in Example 1 has a smaller total strain and better creep resistance.
[0082] The preferred embodiments of this disclosure have been described in detail above with reference to the accompanying drawings. However, this disclosure is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this disclosure, various simple modifications can be made to the technical solutions of this disclosure, and these simple modifications all fall within the protection scope of this disclosure.
[0083] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this disclosure will not describe the various possible combinations separately.
[0084] Furthermore, various different embodiments of this disclosure can be combined in any way, as long as they do not violate the spirit of this disclosure, they should also be regarded as the content disclosed in this disclosure.
Claims
1. A die-cast aluminum alloy material, characterized in that, Based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: 8.5~13 wt% Si, 0.1~1 wt% Mn, 0~0.5 wt% Fe, 1.5~3 wt% Cu, 0.5~2 wt% Mg, 1.0~2.5 wt% Zn, 0.02~0.5 wt% Ti, 0.02~0.08 wt% Sr, 0.02~0.1 wt% Zr, 0~0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al; the die-cast aluminum alloy material also contains 0.01~0.1 wt% Bi element; in the die-cast aluminum alloy material, the content ratio of Cu element to Bi element is less than 40.
2. The die-cast aluminum alloy material according to claim 1, characterized in that, Based on the total weight of the die-cast aluminum alloy material, the die-cast aluminum alloy material comprises: 8.8~12 wt% Si, 0.2~0.8 wt% Mn, 0~0.5 wt% Fe, 1.5~3.0 wt% Cu, 0.065~0.1 wt% Bi, 0.5~2.0 wt% Mg, 1.3~2.3 wt% Zn, 0.02~0.5 wt% Ti, 0.02~0.08 wt% Sr, 0.02~0.1 wt% Zr, 0~0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al.
3. The die-cast aluminum alloy material according to claim 1, characterized in that, In the die-cast aluminum alloy material, the ratio of Cu to Ni is less than 50.
4. The die-cast aluminum alloy material according to claim 1, characterized in that, The intrinsic properties of the die-cast aluminum alloy material include: a yield strength of ≥240MPa, a tensile strength of ≥320MPa, and an elongation of ≥1.5%.
5. A method for preparing die-cast aluminum alloy materials, characterized in that, Includes the following steps: S1. The alloy raw material mixture is smelted in a melting furnace to obtain a first alloy melt. The alloy raw material mixture comprises: 8.5-13 wt% Si, 0.1-1 wt% Mn, 0-0.5 wt% Fe, 1.5-3 wt% Cu, 0.5-2 wt% Mg, 1.0-2.5 wt% Zn, 0.02-0.5 wt% Ti, 0.02-0.08 wt% Sr, 0.02-0.1 wt% Zr, 0-0.1 wt% Ni, less than 0.1 wt% impurities, and the balance Al; the alloy raw material mixture also contains 0.01-0.1 wt% Bi element; the ratio of Cu element to Bi element in the alloy raw material mixture is less than 40. S2. The first alloy melt is subjected to degassing, refining and first slag removal in a converter to obtain the second alloy melt. S3. The second alloy melt is subjected to heat preservation treatment and second slag removal treatment in a machine-side furnace to obtain the third alloy melt. S4. The third alloy melt is subjected to die casting treatment.
6. The method according to claim 5, characterized in that, In step S1, the conditions for the smelting process include: a smelting temperature of 740~760℃, a smelting atmosphere temperature of 700~950℃, and a smelting time of 3~13h.
7. The method according to claim 5, characterized in that, In step S2, the conditions for degassing include: degassing speed of 400~500 r / min, degassing gas source pressure of 0.35~0.45 MPa, degassing temperature of 760~770℃, and degassing time of 8~10 min; The refining process includes: passing nitrogen gas containing refining agent powder into the first alloy melt after degassing treatment for a first refining, and passing nitrogen gas containing refining agent powder again for a second refining. The first slag removal process includes removing slag using slag removal tools.
8. The method according to claim 5, characterized in that, In step S3, the conditions for the heat preservation treatment include: heat preservation temperature of 660~680℃ and heat preservation time of 30~40min; The second slag removal process includes removing slag using slag removal tools.
9. The method according to claim 5, characterized in that, In step S4, the conditions for the die casting process include: casting pressure above 60 MPa, high speed above 3.5 m / s, vacuum degree below 100 mbar, aluminum liquid temperature of 660~680℃, mold coating temperature of 120~150℃, and injection delay time of less than 1 s.
10. The die-cast aluminum alloy material prepared by the method according to any one of claims 5 to 9.
11. An automotive structural component, characterized in that, Includes die-cast aluminum alloy material, wherein the die-cast aluminum alloy material is the die-cast aluminum alloy material as described in any one of claims 1 to 4 and 10.
Citation Information
Patent Citations
Heat-treatment-free die-casting aluminum alloy material, preparation method thereof and automobile structural part
CN116752018A
Aluminum alloy and preparation method and application of aluminum alloy
CN106811630A
As-cast high-strength high-toughness die-casting aluminum-silicon alloy and preparation method thereof
CN115976356A
Heat-treatment-free die-casting aluminum alloy material, preparation method thereof and automobile structural part
CN117568671A