Conductive agent and preparation method thereof, and electronic component using the same
Through the combination of conductive materials, glass and organic color spreader, the chemical composition and particle size of glass are optimized, and the problem of poor performance of the conductive layer during electroplating and welding is solved, and the high density and acid-base corrosion resistance of the conductive layer are achieved. , improves the overall performance and welding characteristics of electronic components.
Patent Information
- Application Number
- CN202410236244.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-02-29
AI Technical Summary
After the existing conductive agent is sintered, the conductive layer formed in the electroplating and welding process is poor, making it difficult to meet the comprehensive performance and service life requirements of electronic components.
By using a combination of conductive materials, glass and organic color spreader, the density and acid-base corrosion resistance of the conductive layer are improved by optimizing the chemical composition and particle size of the glass, and ensuring the good performance of the conductive layer during electroplating and welding.
The formed conductive layer has excellent electroplating and welding characteristics, which reduces welding defects and structural weaknesses, and improves the overall performance and heat resistance of electronic components.
Smart Images

Figure BDA0004726283150000041 
Figure BDA0004726283150000051 
Figure BDA0004726283150000062
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic functional materials, and in particular, relates to a conductive agent and a preparation method thereof, and an electronic component using the conductive agent. Background Art
[0002] Conductive agents are widely used in surface metallization or electrode connection of electronic components. The conductive agent is fixed or fully flattened on the surface of the electronic device, and then sintered and solidified to form a conductive layer. Especially in electronic components and electrical products such as dielectric ceramic capacitors, resistors, inductors, buzzers, solar cells, ceramic filters, and automobile rear windshield defogger lines, conductive agents will affect the comprehensive performance and service life of the products.
[0003] In the actual preparation process, after the conductive agent is sintered and solidified, it is usually necessary to connect other electronic devices through electroplating and welding to achieve power supply. Therefore, the sintered conductive layer needs to have excellent electroplating and welding properties.
[0004] Therefore, it is necessary to seek a conductive agent so that the conductive layer formed by curing has excellent electroplating properties and welding properties. Summary of the invention
[0005] The object of the present invention is to provide a conductive agent and a preparation method thereof, and an electronic component using the conductive agent, wherein the conductive layer formed by the conductive agent has excellent electroplating properties and welding properties.
[0006] According to one aspect of the present invention, there is provided a conductive agent, comprising a conductive material, glass, and an organic color developer, wherein the conductive material accounts for no less than 50 wt% of the conductive agent composition; the chemical composition of the glass comprises silicon dioxide, zinc oxide, boron oxide, sodium oxide, titanium dioxide, zirconium dioxide, and fluorine; in the glass, the content of silicon dioxide is no more than 45 wt%, the content of zinc oxide is no more than 25 wt%, the content of boron oxide is no more than 15 wt%, the content of sodium oxide is no less than 5 wt%, the content of titanium dioxide is 1-6 wt%, the content of zirconium dioxide is no less than 2 wt%, and the content of fluorine is no more than 2 wt%; and calculated by mass ratio, glass: conductive material = 0.03-0.15:1.
[0007] The conductive agent includes conductive materials, glass, and organic color developers, wherein the conductive material is used as the conductive phase in the conductive agent to provide a conductive channel; the organic color developer is used as an organic carrier in the conductive agent, which is conducive to the smooth coating of the conductive agent on the substrate layer; glass is used as the bonding phase of the conductive agent to bond the conductive material inside the conductive layer, fix the conductive layer formed by the conductive agent, and the substrate layer coated with the conductive agent. Therefore, the type of glass will affect the density of the conductive layer, the bonding effect between the conductive layer and the substrate layer, and in the actual preparation process, after the conductive agent is sintered and solidified, it is usually necessary to cover the surface of the solidified conductive layer with a layer of electroplating by electroplating. In other words, the conductive layer needs to be immersed in a strongly acidic, weakly acidic or strongly alkaline plating solution. Furthermore, the electroplated conductive layer and the substrate layer need to be connected to the electronic device by welding and other methods to form an electronic product with certain functions.
[0008] This solution combines silicon dioxide (SiO2), zinc oxide (ZnO), boron oxide (B2O3), sodium oxide (Na2O), titanium dioxide (TiO2), zirconium dioxide (ZrO2), and fluorine (F) in the above-mentioned mass ratio, and utilizes the synergistic effect between various materials to improve the corrosion resistance of the glass, thereby improving the electroplating and welding characteristics of the conductive layer formed by the conductive agent, and when the feed ratio of glass to conductive material is 0.03 to 0.15:1, the conductive layer formed by the conductive agent can have good adhesion to the substrate layer and electroplating characteristics at the same time. By using the above-mentioned glass to prepare the conductive agent, the conductive layer formed by the conductive agent not only has good density, but also has excellent acid and alkali corrosion resistance. Therefore, the conductive layer is not easily penetrated or corroded by the plating solution, which can reduce the structural weaknesses on the surface of the conductive layer, improve the electroplating and welding characteristics of the conductive layer, and reduce the welding defect rate of the product.
[0009] Preferably, the chemical composition of the glass also includes calcium oxide, and the content of calcium oxide is not higher than 6wt% and the content of sodium oxide is 5-10wt% calculated by mass percentage. Among the existing welding methods, reflow soldering and wave soldering are the most extensive and mature, but the welding temperature required for reflow soldering and wave soldering is relatively high, so there are certain welding heat resistance requirements for the conductive layer. By introducing calcium oxide into the glass and optimizing the upper limit of the content of calcium oxide (CaO) and sodium oxide (Na2O), the conductive layer formed by the conductive agent can be made less likely to crack under high temperature environment under the premise that the conductive layer has high electroplating characteristics and welding characteristics. If the content of CaO is higher than 6wt% or the content of Na2O is higher than 10wt%, the reaction activity between the conductive agent containing the glass and the substrate layer is too high, and it is easy to over-react under the same reaction conditions. If there is an over-reaction, an excess reaction layer is easily formed between the conductive layer and the substrate layer. During the welding process, the areas where there is excess reaction layer will exert thermal stress on the base material layer and the conductive layer, causing cracks in the conductive layer and the base material layer under high temperature environment, that is, the welding heat resistance is poor.
[0010] Preferably, calculated by mass percentage, the chemical composition of the glass includes 35-45wt% silicon dioxide, 15-25wt% zinc oxide, 5-15wt% boron oxide, 2-8wt% zirconium dioxide, and 2-6wt% calcium oxide. By optimizing the minimum content of silicon dioxide (SiO2), zinc oxide (ZnO), boron oxide (B2O3), calcium oxide (CaO) and the maximum content of zirconium dioxide (ZrO2), not only the chemical stability and mechanical strength of the conductive layer can be improved, but also the adhesion of the conductive layer to the substrate layer can be improved. Among them, when the chemical composition of the glass meets the above conditions, the softening temperature of the glass is moderate, which can improve the reaction activity between the conductive agent and the substrate layer and increase the adhesion of the conductive layer to the substrate layer. If the content of SiO2, ZnO, B2O3, and CaO is too low or the content of ZrO2 is too high in the chemical composition of the glass, the reaction activity between the conductive agent composition and the substrate layer will decrease, and there will be a situation where the conductive layer and the substrate layer are locally unevenly stressed, which is prone to bending.
[0011] Preferably, the average particle size of the glass is 2 to 5 μm.
[0012] Preferably, the method for preparing glass comprises the following operations: weighing raw materials for preparing glass according to quantity, keeping the raw materials for preparing glass at a temperature of 1400-1600°C for 0.5-1.5 hours to obtain a melt; transferring the melt to an environment of 0-30°C for cooling and shaping to obtain glass. Through the above operation, glass with a stable structure and good compatibility with conductive materials and organic color developers can be obtained. By adjusting the reaction temperature and reaction time, the occurrence of side reactions can be reduced, which is conducive to controlling the morphology of the final product.
[0013] Preferably, the average particle size of the conductive material is 0.3 to 10 μm. The conductive agent composition prepared by using the conductive material in the above-mentioned particle size range can not only form a conductive layer with good conductivity, but also has good structural density and structural stability of the conductive layer. When the above-mentioned conductive material is combined with glass with an average particle size of 2 to 5 μm to prepare a conductive agent composition, the conductive agent composition can form a conductive layer with a smooth surface and a dense structure, which is convenient for subsequent electroplating or welding. If the average particle size of the conductive material is too small, the conductive material is prone to shrinkage during the sintering and curing process to form a conductive layer, resulting in cracks in the conductive layer, and the plating solution will penetrate into the cracks, thereby affecting the structural stability of the conductive layer. If the average particle size of the conductive material is too large, gaps are likely to exist between the conductive materials and between the conductive material and the glass, resulting in a decrease in the density of the conductive layer, and it is also easy to cause the plating solution to penetrate into the conductive layer, resulting in a decrease in the bonding effect.
[0014] Preferably, the conductive material includes at least one of silver (Ag), gold (Au), copper (Cu), nickel (Ni), platinum (Pt), and palladium (Pd).
[0015] Preferably, the conductive material accounts for 60-80 wt % of the conductive agent.
[0016] More preferably, the conductive material accounts for 70 wt % in the conductive agent.
[0017] Preferably, the organic vehicle comprises a resin and a solvent.
[0018] Preferably, calculated by mass ratio, resin:solvent=60-80:20-40.
[0019] More preferably, calculated by mass ratio, resin:solvent=70:30.
[0020] According to a second aspect of the present invention, a method for preparing the above-mentioned conductive agent is provided, comprising the following operations: weighing raw materials for preparing the conductive agent according to amount, mixing the raw materials for preparing the conductive agent at a temperature of 25 to 35° C., and obtaining the conductive agent. The preparation process of the conductive agent provided in this solution has simple steps, convenient operation, mild conditions, and good economic benefits.
[0021] According to a third aspect of the present invention, there is provided an electronic component comprising a base component and a conductive layer, wherein the conductive layer is made of the conductive agent according to any one of claims 1 to 8. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0023] Example 1
[0024] (1) Preparation of glass
[0025] Calculated by mass percentage, the raw materials used to prepare glass include: SiO2, ZnO, B2O3, Na2O, TiO2, ZrO2, F, and CaO. The above materials are mixed according to the chemical composition shown in Table 1, and SiO2 is used as a variable to prepare the glass of each experimental group and control group in this embodiment. In this embodiment, the experimental groups or control groups set are marked as experimental group 1-1, experimental group 1-2, experimental group 1-3, experimental group 1-4, and control group 1, respectively.
[0026] Table 1. Chemical composition of each glass in Example 1
[0027]
[0028] The method for preparing glass includes the following operations:
[0029] Weighing raw materials for preparing glass according to amount, and keeping the raw materials for preparing glass at a temperature of 1500° C. for 1 hour to obtain a melt;
[0030] The melt was transferred to water at 20°C for water cooling and cooling to obtain glass. The glass was then crushed using a ball mill to obtain glass with an average particle size of 2 μm.
[0031] (2) Preparation of conductive agent
[0032] Calculated by mass percentage, the raw materials used to prepare the conductive agent include: 70wt% conductive material, 4.9wt% of the above-mentioned glass, and 25.1wt% organic color developer. Among them, the conductive material uses copper powder with an average particle size of 2μm, and the organic color developer uses resin and solvent, and the mass ratio of resin to solvent is 7:3. In other embodiments, the type of conductive material, the type of resin and solvent, and the ratio of resin to solvent can be adjusted according to different needs, provided that the normal use of the conductive agent is not affected.
[0033] The preparation method of the conductive agent includes the following operations: weighing raw materials for preparing the conductive agent according to quantity, putting the raw materials for preparing the conductive agent into a three-roll pulping machine, and kneading at a temperature of 25 to 35° C. to mix evenly to obtain the conductive agent.
[0034] Example 2
[0035] This example refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this example and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 2. This example uses the content of ZnO as a variable to prepare the glass of each experimental group and control group in this example. In this example, the experimental groups or control groups set are marked as experimental group 2-1, experimental group 2-2, experimental group 2-3, experimental group 2-4, and control group 2. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0036] Table 2. Chemical composition of each glass in Example 2
[0037]
[0038]
[0039] Example 3
[0040] This example refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this example and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 3. This example uses the content of B2O3 as a variable to prepare the glass of each experimental group and control group in this example. In this example, the experimental groups or control groups set are marked as experimental group 3-1, experimental group 3-2, experimental group 3-3, experimental group 3-4, and control group 3. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0041] Table 3. Chemical composition of each glass in Example 3
[0042]
[0043] Example 4
[0044] This example refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this example and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 4. This example uses the content of Na2O as a variable to prepare the glass of each experimental group and control group in this example. In this example, the experimental groups or control groups set are marked as experimental group 4-1, experimental group 4-2, experimental group 4-3, experimental group 4-4, and control group 4. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0045] Table 4. Chemical composition of each glass in Example 4
[0046]
[0047]
[0048] Example 5
[0049] This example refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this example and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 5. This example uses the content of TiO2 as a variable to prepare the glass of each experimental group and control group in this example. In this example, the experimental groups or control groups set are marked as experimental group 5-1, experimental group 5-2, experimental group 5-3, experimental group 5-4, and control group 5. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0050] Table 5. Chemical composition of each glass in Example 5
[0051]
[0052] Example 6
[0053] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this embodiment and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 6. This embodiment uses the content of ZrO2 as a variable to prepare the glass of each experimental group and control group in this embodiment. In this embodiment, the experimental groups or control groups set are marked as experimental group 6-1, experimental group 6-2, experimental group 6-3, experimental group 6-4, and control group 6. The remaining raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0054] Table 6. Chemical composition of each glass in Example 6
[0055]
[0056]
[0057] Example 7
[0058] This embodiment refers to the preparation method provided by experimental group 2-3 to prepare the conductive agent. The difference between this embodiment and experimental group 2-3 is that: in the process of preparing glass, the raw materials used for preparing glass are used according to the chemical composition shown in Table 7. This embodiment uses the content of F as a variable to prepare the conductive agents of each experimental group and control group in this embodiment. In this embodiment, the experimental groups or control groups set are marked as experimental group 7-1, experimental group 7-2, and control group 7, respectively. The rest of the raw material ratios and preparation methods are strictly consistent with those of experimental group 2-3.
[0059] Table 7. Composition ratio of each conductive agent in Example 7
[0060]
[0061] Example 8
[0062] This example refers to the preparation method provided in Example 1 to prepare a conductive agent. The difference between this example and Example 1 is that in the process of preparing glass, the raw materials used to prepare glass are used according to the chemical composition shown in Table 8. This example uses the content of CaO as a variable to prepare the conductive agents of each experimental group and control group in this example. In this example, the experimental groups or control groups set are marked as experimental group 8-1, experimental group 8-2, experimental group 8-3, experimental group 8-4, and experimental group 8-5, respectively. The remaining raw material ratios and preparation methods are strictly consistent with those in Example 1.
[0063] Table 8. Composition ratio of each conductive agent in Example 8
[0064]
[0065]
[0066] Example 9
[0067] This embodiment refers to the preparation method provided by Experimental Group 2-3 to prepare the conductive agent. The difference between this embodiment and Experimental Group 2-3 is that in the process of preparing the conductive agent, the type or average particle size of the conductive material is adjusted according to the conductive material shown in Table 9 to prepare the conductive agent of each experimental group and control group in this embodiment. In this embodiment, the experimental groups or control groups set are marked as Experimental Group 9-1, Experimental Group 9-2, and Experimental Group 9-3, respectively. The rest of the raw material ratios and preparation methods are strictly consistent with Experimental Group 2-3, especially the chemical group of the glass is strictly consistent with Experimental Group 2-3.
[0068] Table 9. Conductive materials of each conductive agent in Example 9
[0069] Group Conductive material type Average particle size of conductive material Experimental Group 9-1 Copper powder 0.3μm Experimental Group 9-2 Copper powder 7μm Experimental Group 9-3 Copper powder 10μm
[0070] Test Case
[0071] Test object: The conductive agent provided in Examples 1 to 9 was coated on a 1203 size Ni internal electrode stacked capacitor by dip coating, and dried, and then sintered at a set temperature of 800°C for 10 minutes under N2 atmosphere to solidify the conductive agent into a conductive layer. The internal electrode stacked capacitor coated with the conductive agent was then electroplated with Ni and Sn to obtain a sample, which was used as a test object.
[0072] Test items and test methods:
[0073] (1) Adhesion strength: The test object is welded on a PCB substrate with wiring (substrate for adhesion strength, material: glass epoxy resin), and pressure is applied from the side at a speed of 1 mm / s. The measured breaking strength is the adhesion strength. The number of samples is 30 for each condition, and the average value is taken.
[0074] (2) Bending failure rate: Solder the test object on the wiring PCB substrate (thickness: 1.6mm) used for the bending test, and bend the substrate 2mm for 10 seconds. Then grind the test object and observe the cross section to see if there are any cracks on the test object. The number of test samples is 30 for each condition, and the bending failure rate is calculated. Bending failure rate = (number of test objects with cracks / total number of test samples) × 100%.
[0075] (3) Soldering characteristics: At 245°C, immerse the test object in a solder bath containing molten Sn-3.5Ag-0.5Cu solder for 5 seconds. The test object is judged to be qualified if the creeping area is above 95%. The number of test samples is 30 for each condition, and the soldering defect rate is calculated. Soldering defect rate = (number of test objects with unqualified creeping area / total number of test samples) × 100%.
[0076] (4) Soldering heat resistance characteristics: Immerse the test object in a molten solder bath for 3 seconds at 350°C. The solder is molten Sn-3.5Ag-0.5Cu. Observe the surface of the test object to determine whether there are cracks. The number of test samples is 30 for each condition, and the welding heat resistance failure rate is calculated. Welding heat resistance failure rate = (number of test objects with cracks / total number of test samples) × 100%.
[0077] Test results: The test results are shown in Table 10.
[0078] Table 10. Test results of each subject
[0079]
[0080]
[0081] Result analysis:
[0082] The conductive agents provided in Examples 1 to 9 were compared. As shown in Table 10, compared with the corresponding test performances of Control Groups 1 to 7, the conductive layers formed by the conductive agents used in the other experimental groups have excellent electroplating properties and soldering properties, among which the conductive agents provided in Experimental Groups 2-3 have the best comprehensive properties. After Ni and Sn electroplating, not only is the adhesion strength between the conductive layer and the substrate layer large and not easy to bend, but the conductive layer also has good welding properties and welding heat resistance properties.
[0083] Furthermore, in Example 1, Example 3, and Examples 5 to 8, the welding failure rate of the other experimental groups is smaller than that of the conductive layer formed by the conductive agent in Control Group 1, Control Group 3, and Control Groups 5 to 8. This shows that if the content of silicon dioxide (SiO2), boron oxide (B2O3), titanium dioxide (TiO2), and fluorine (F) is too high or the content of zirconium dioxide (ZrO2) is too low, the glass is easily corroded by the electroplating solution, resulting in the conductive layer formed by the conductive composition being prone to structural weaknesses after electroplating, and also prone to bending.
[0084] In Example 2 and Example 4, the welding failure rate of other experimental groups is smaller than the test performance of Control Group 2 and Control Group 4 in Table 10. This shows that if the content of zinc oxide (ZnO) is too high or the content of sodium oxide (Na2O) is too low, the glass is prone to crystallization reaction, thereby affecting the overall stability of the conductive layer, and easily leading to poor welding or poor electroplating effect in subsequent processing.
[0085] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A conductive agent, It is characterized in that It comprises a conductive material, glass, and an organic color developer, wherein the conductive material accounts for no less than 50wt% of the conductive agent composition; The chemical composition of the glass includes silicon dioxide, zinc oxide, boron oxide, sodium oxide, titanium dioxide, zirconium dioxide, and fluorine; in the glass, the content of silicon dioxide is not higher than 45wt%, the content of zinc oxide is not higher than 25wt%, the content of boron oxide is 5-15wt%, the content of sodium oxide is not lower than 5wt%, the content of titanium dioxide is 1-6wt%, the content of zirconium dioxide is 2-10wt%, and the content of fluorine is not higher than 2wt%; And calculated according to the mass ratio, the glass: the conductive material = 0.03-0.15:
1.
2. The conductive agent according to claim 1, It is characterized in that The chemical composition of the glass also includes calcium oxide, and calculated by mass percentage, the content of calcium oxide is no more than 6wt%, and the content of sodium oxide is 5-10wt%.
3. The conductive agent according to claim 2, It is characterized in that Calculated by mass percentage, the chemical composition of the glass includes 35-45wt% silicon dioxide, 15-25wt% zinc oxide, 5-15wt% boron oxide, 2-8wt% zirconium dioxide, and 2-6wt% calcium oxide.
4. The conductive agent according to claim 1, It is characterized in that The average particle size of the glass is 2 to 5 μm.
5. The conductive agent according to any one of claims 1 to 4, It is characterized in that The method for preparing the glass comprises the following operations: Weighing raw materials for preparing the glass according to amount, and keeping the raw materials for preparing the glass at a temperature of 1400 to 1600° C. for 0.5 to 1.5 hours to obtain a melt; The melt is transferred to an environment of 0-30° C. to be cooled and shaped, thereby obtaining the glass.
6. The conductive agent according to claim 1, It is characterized in that The average particle size of the conductive material is 0.3-10 μm.
7. The conductive agent according to claim 6, It is characterized in that The conductive material includes at least one of silver, gold, copper, nickel, platinum and palladium.
8. The conductive agent according to any one of claims 1 to 4, 6 to 7, It is characterized in that The conductive material accounts for 60-80 wt % of the conductive agent.
9. A method for preparing the conductive agent according to any one of claims 1 to 8, It is characterized in that The method comprises the following operations: weighing raw materials for preparing the conductive agent according to quantity, mixing the raw materials for preparing the conductive agent at a temperature of 25 to 35° C., and obtaining the conductive agent.
10. An electronic component, It is characterized in that The invention comprises a basic component and a conductive layer, wherein the conductive layer is made of the conductive agent according to any one of claims 1 to 8.