Cylindrical battery for improving negative electrode silicon-doped power battery cycle and preparation method thereof, and battery module containing the cylindrical battery
By using composite negative electrode materials of silicon oxide, porous silicon carbon and superionic conductor layers in lithium-ion batteries, the problem of capacity fading caused by expansion and reaction of silicon-doped materials in lithium-ion batteries is solved, and the cycle performance and energy of the battery are improved. density.
Patent Information
- Application Number
- CN202410451778.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-16
AI Technical Summary
The silicon-doped anode material in existing lithium-ion batteries expands in volume and reacts with the electrolyte during charge and discharge, resulting in battery capacity attenuation, and fails to effectively solve the expansion problem when the electrolyte comes into contact with silicon oxide.
A composite negative electrode material composed of a silicon oxide layer, a porous silicon carbon layer and a superionic conductor layer is used. These layers are coated sequentially through coating equipment to form a protective layer to block the electrolyte, reduce expansion and side reactions, and bond through The agent improves the conductivity of lithium ions.
It improves the cycle performance and energy density of the battery, extends the service life of the battery, reduces expansion and side reactions, and enhances the protective effect of the negative electrode material.
Smart Images

Figure CN118053980B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of lithium batteries, and in particular to a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery, a preparation method thereof, and a battery module containing the cylindrical battery. Background Art
[0002] With the rapid development of the new energy industry, the application of large cylindrical batteries in the power market has gradually increased, and they have a certain share in the power battery market.
[0003] Large cylindrical batteries have smaller internal resistance and faster charging speed due to their full-ear structure, and are currently being rapidly promoted in the field of power batteries. Currently, in the application direction of long-cycle power batteries, silicon-doped negative electrodes of ternary lithium-ion batteries are the best choice for achieving high energy density.
[0004] However, in the actual application of silicon-doped large cylindrical power batteries, the volume of silicon materials expands during the process of lithium insertion and extraction, making the surface of silicon particles easily damaged. The silicon material on the surface of the negative electrode is constantly damaged during the charging and discharging process, causing the battery capacity to decay continuously. In the current silicon negative electrode battery system, not only is there the problem of silicon volume expansion, but the silicon material also reacts chemically with the electrolyte, continuously consuming the limited lithium source, silicon source and electrolyte in the battery system, thus causing battery failure and accelerating the battery capacity decay.
[0005] For example, the comparative document CN201910228636.4 discloses a silicon oxide composite negative electrode material with a gradient structure, and its preparation method and application. The negative electrode material includes a core-shell structure consisting of a silicon dioxide layer, a silicon oxide material layer (SiOx) and a carbon coating layer distributed from the inside to the outside. The silicon oxide material layer is a layered structure of at least two layers, and the molar ratio of Si:O in the layered structure gradually increases from the inside to the outside. Although the above-disclosed technical solution uses a gradient structure to make the stress of silicon oxide more uniform when the volume expands during charging, the solution does not solve the problem that when the electrolyte contacts silicon oxide, silicon oxide reacts with the electrolyte during the battery cycle to produce expansion.
[0006] For example, the comparative document CN202311291991.9 discloses a multi-layered composite negative electrode material and a preparation method thereof. The multi-layered composite negative electrode material includes, from the inside to the outside, a core, a first coating layer, and a second coating layer; the core includes silicon nanoparticles, the first coating layer includes silicon oxide, and the second coating layer is a carbon layer; the carbon layer is derived from the pyrolysis of heavy oil. Although the above-disclosed technical solution uses silicon oxide as a transition layer, combines the advantages of silicon, silicon oxide and carbon layer, retains the high lithium storage capacity of the silicon negative electrode, and utilizes the high capacity and relatively small volume expansion rate of silicon oxide, the solution also does not solve the problem that when the electrolyte contacts silicon oxide, silicon oxide reacts with the electrolyte during the battery cycle to produce expansion. Summary of the invention
[0007] The purpose of the present disclosure is to overcome the deficiencies in the prior art and to provide a cylindrical battery for improving the cycle of negative electrode doped silicon power batteries by improving the expansion of negative electrode materials, reducing the reaction with electrolyte and increasing the battery cycle, and a preparation method thereof, as well as a battery module containing the cylindrical battery.
[0008] The purpose of this disclosure is achieved through the following technical solutions:
[0009] A method for preparing a cylindrical battery for improving the cycle of a negative electrode doped with silicon power battery, characterized in that it is used to prepare a cylindrical battery for improving the cycle of a negative electrode doped with silicon power battery, and the cylindrical battery for improving the cycle of a negative electrode doped with silicon power battery comprises a negative electrode sheet, a positive electrode sheet, a diaphragm and a shell, wherein the negative electrode sheet, the diaphragm and the positive electrode sheet are wound to form a roll core, the roll core is built into the shell, and the shell is also filled with an electrolyte, and the electrolyte is used to infiltrate the roll core; the negative electrode sheet comprises a silicon oxide layer, a porous silicon carbon layer, a superionic conductor layer and a negative electrode current collector, the silicon oxide layer is coated on the negative electrode current collector, the porous silicon carbon layer is coated on the silicon oxide layer, and the superionic conductor layer is coated on the negative electrode current collector. The sub-conductor layer is coated on the porous silicon carbon layer; the porous silicon carbon layer is used to separate the silicon oxide layer, and the superionic conductor layer is used to separate the porous silicon carbon layer and the electrolyte; the number of the silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer is two, the two silicon oxide layers are respectively coated on both sides of the negative electrode current collector, the two porous silicon carbon layers are respectively coated on the corresponding silicon oxide layers, and the two superionic conductor layers are respectively coated on the corresponding porous silicon carbon layers; the superionic conductor layer is coated by continuous coating, and the thickness of the superionic conductor layer is 1um-2um; the preparation method comprises the following steps:
[0010] a slurry for making a silicon oxide layer;
[0011] The slurry of silicon dioxide layer includes the following components in different weights:
[0012] Active material graphite Gr: 88.4;
[0013] Silicon dioxide: 8%;
[0014] Polyacrylate lithium PAA-Li: 1.5%;
[0015] Sodium carboxymethyl cellulose CMC2200: 0.5%;
[0016] Conductive carbon black SP: 0.5%;
[0017] Single-walled carbon tubes SWCNTs: 0.4%;
[0018] Styrene butadiene rubber emulsion SBR: 0.7%;
[0019] Silicon dioxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tubes SWCNTs and styrene-butadiene rubber latex SBR are placed in a stirring tank for mixing and stirring; and the viscosity value of the silicon dioxide layer is tested before the stirred silicon dioxide layer is stored in a transfer tank;
[0020] a slurry for making a porous silicon carbon layer;
[0021] The slurry of the porous silicon carbon layer includes the following components in various weights:
[0022] Active material graphite Gr: 87.1%;
[0023] Porous silicon carbon: 10%;
[0024] Polyacrylate lithium PAA-Li: 1.5%;
[0025] Sodium carboxymethyl cellulose CMC2200: 0.5%;
[0026] Single-walled carbon tubes SWCNTs: 0.4%;
[0027] Styrene butadiene rubber emulsion SBR: 0.7%;
[0028] The porous silicon carbon layer, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber latex SBR are placed in a stirring tank for mixing and stirring; the stirred porous silicon carbon layer is then stored in a transfer tank; the solid content of the porous silicon carbon layer is adjusted according to the viscosity value of the silicon oxide layer, so that the viscosity value of the porous silicon carbon layer is close to the viscosity value of the silicon oxide layer;
[0029] The slurry of the superionic conductor layer is prepared, and the slurry of the superionic conductor layer includes the following components in various weights:
[0030] Lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6 (PO4) 3: 96%;
[0031] Adhesive: 2.5%;
[0032] Styrene butadiene rubber emulsion SBR: 1.5%;
[0033] The adhesive comprises lithium polyacrylate PAA-Li and lithium carboxymethyl cellulose CMC-Li, and the mass ratio of the lithium polyacrylate PAA-Li to the lithium carboxymethyl cellulose CMC-Li is 1.5:1;
[0034] Before lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 is put into a stirring tank for mixing and stirring with a binder and styrene-butadiene rubber emulsion SBR to form a superionic conductor layer, the stirred superionic conductor layer is passed through a transfer tank, and then the solid content of the superionic conductor layer is adjusted according to the viscosity value of the porous silicon carbon layer, so that the viscosity value of the superionic conductor layer is close to that of the porous silicon carbon layer;
[0035] When preparing the silicon oxide layer, when silicon oxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene butadiene rubber emulsion SBR are placed in a stirring tank for mixing and stirring, the mixed slurry is added for mixing to increase the proportion of the silicon oxide layer in the slurry and increase the solid content of the silicon oxide layer in the slurry mixture; when preparing the porous silicon carbon layer, the porous silicon carbon layer is mixed with lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene butadiene rubber emulsion SB When R is put into a stirring kettle for mixing and stirring, the slurry is added for mixing, thereby increasing the solid content of the porous silicon carbon layer in the slurry mixture; when making a superionic conductor layer, lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3, an adhesive, and styrene-butadiene rubber emulsion SBR are put into a stirring kettle for mixing and stirring to make a superionic conductor layer, and the slurry is added for mixing to increase the proportion of the superionic conductor layer in the slurry, thereby increasing the solid content in the superionic conductor layer slurry mixture; the solid content of the silicon oxide layer, the porous silicon carbon layer, and the superionic conductor layer slurry mixture is controlled between 40% and 55%;
[0036] The slurry of the silicon oxide layer, the slurry of the porous silicon carbon layer and the slurry of the superionic conductor layer are simultaneously coated in multiple layers by a coating device, the slurry of the silicon oxide layer is coated on the negative electrode current collector, the slurry of the porous silicon carbon layer is coated on the corresponding slurry surface of the silicon oxide layer, and the slurry of the superionic conductor layer is coated on the corresponding slurry surface of the porous silicon carbon layer; the capacity ratio of the porous silicon carbon layer to the silicon oxide layer is 0.05-0.25;
[0037] The coating equipment is provided with a first coating port, a second coating port and a third coating port, the first coating port is used for coating a silicon oxide layer, the second coating port is used for coating a porous silicon carbon layer, and the third coating port is used for coating a superionic conductor layer. The first coating port, the second coating port and the third coating port are arranged in sequence, and the interval between the first coating port, the second coating port and the third coating port is 30 cm-40 cm. A suitable interval is set so that the interval time of sequentially coating the silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer is short;
[0038] During the coating process, the first coating port, the second coating port and the third coating port respectively coat different amounts of silicon dioxide layer, porous silicon carbon layer and superionic conductor layer; it is necessary to control the first coating port, the second coating port and the third coating port of the coating equipment to be debugged respectively, the coating device controls the output thickness by controlling the size of the output port, and the coating device controls the pressure of the output material and the flow rate of the output slurry by controlling the mass volume ratio of the porous silicon carbon layer, the silicon dioxide layer and the superionic conductor layer. During coating, the temperature of the silicon dioxide layer, the porous silicon carbon layer and the superionic conductor layer is controlled between 15°C and 35°C to enable the coating device to discharge materials smoothly; the empty foil is placed at the first coating port for coating, and the surface density of the silicon dioxide layer coated at the first coating port is adjusted; the empty foil is then placed at the second coating port, and the surface density of the porous silicon carbon layer coated at the second coating port is adjusted; the empty foil is then placed at the third coating port, and the third coating port is adjusted to coat the superionic conductor layer;
[0039] The cross sections of the first coating port, the second coating port and the third coating port are gradually reduced, and the extrusion pressure of the first coating port, the second coating port and the third coating port is gradually reduced;
[0040] The distance between the first coating port and the empty foil is a first distance, the distance between the second coating port and the empty foil is a second distance, and the distance between the third coating port and the empty foil is a third distance; the first distance is greater than the second distance, and the second distance is greater than the third distance;
[0041] The negative electrode current collector coated with the slurry of the silicon oxide layer, the slurry of the porous silicon carbon layer and the slurry of the super ion conductor layer is baked at high temperature to form the negative electrode sheet in which the silicon oxide layer is coated on the negative electrode current collector, the porous silicon carbon layer is coated on the silicon oxide layer, and the super ion conductor layer is coated on the porous silicon carbon layer;
[0042] The negative electrode sheet, the separator and the positive electrode sheet are stacked and then wound to form the winding core;
[0043] After flattening and shaping the tabs of the winding core, the winding core is placed in the shell for welding, and a battery cell is obtained after welding;
[0044] The battery cell is subjected to a process of injecting liquid into the battery cell;
[0045] The battery core is welded and sealed to obtain the cylindrical battery for improving the cycle of the negative electrode doped silicon power battery.
[0046] A battery module comprises the cylindrical battery for improving the cycle of a negative electrode doped silicon power battery prepared by the method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery described in the above embodiment.
[0047] Compared with the prior art, the present invention has the following advantages, including but not limited to:
[0048] 1. The above-mentioned cylindrical battery for improving the cycle of negative electrode doped silicon power battery and its preparation method, as well as the battery module containing the cylindrical battery, have a higher gram capacity of the silicon oxide layer on the negative electrode sheet, which increases the energy density of the battery. Since the porous silicon carbon layer is coated on the silicon oxide layer, that is, the porous silicon carbon layer forms a protective layer on the surface of the silicon oxide layer, the silicon oxide layer is blocked from direct contact with the electrolyte, thereby protecting the silicon oxide layer and reducing the expansion of the silicon oxide layer caused by the reaction. Compared with the silicon oxide layer, the porous structure of the porous silicon carbon layer is not easy to expand. Furthermore, since the superionic conductor layer is coated on the porous silicon carbon layer, the superionic conductor layer separates the porous silicon carbon layer from the electrolyte, reducing the side reaction between the porous silicon carbon layer and the electrolyte, thereby improving the cycle performance and capacity of the battery.
[0049] 2. The silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer are coated on the negative electrode current collector from the inside to the outside in sequence by means of a coating device, and the silicon oxide layer slurry, the porous silicon carbon layer slurry and the superionic conductor layer slurry are dried simultaneously during preparation, so that the drying speeds of the silicon oxide layer, the porous silicon carbon layer and the superionic conductor are almost the same, thereby making the negative electrode current collector, the silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer have better bonding strength, the porous silicon carbon layer has a better protection effect on the silicon oxide layer, and the superionic conductor layer has a better effect of separating the porous silicon carbon layer and the electrolyte, thereby improving the cycle performance of the battery.
[0050] 3. By using adhesives such as carboxymethyl cellulose lithium CMC-Li and polyacrylate lithium PAA-Li, compared with traditional sodium salt adhesives, the permeability of lithium ions in the silicon oxide layer, porous silicon carbon layer, and superionic conductor layer is increased, thereby improving the discharge performance of cylindrical batteries in the negative electrode silicon-doped power battery cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0052] Figure 1 A schematic diagram of the structure of a negative electrode sheet of a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery according to an embodiment;
[0053] Figure 2 A schematic structural diagram of a negative electrode sheet of a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery according to another embodiment;
[0054] Figure 3 A schematic diagram of the structure of a negative electrode sheet of a cylindrical battery in a ratio;
[0055] Figure 4 A flowchart of the steps of a method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery according to an embodiment;
[0056] Figure 5 It is a comparison chart of the capacity retention rate of the embodiment and the comparative example after 300cls cycle;
[0057] Figure 6 A comparison diagram of the thickness expansion rate of the negative electrode of the embodiment and the comparative example;
[0058] Figure 7 It is a comparison chart of the remaining capacity of the embodiment and the comparative example after 7-day storage at 60°C;
[0059] Figure 8 It is a comparison chart of -20℃ 1C discharge of the embodiment and the comparative example. DETAILED DESCRIPTION
[0060] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.
[0061] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0062] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present disclosure belongs. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0063] In order to better understand the technical solutions and beneficial effects of the present invention, the present invention is further described in detail below in conjunction with specific embodiments:
[0064] like Figure 1 As shown, a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery according to an embodiment of the present disclosure includes a negative electrode sheet, a positive electrode sheet, a diaphragm and a shell, wherein the negative electrode sheet, the diaphragm and the positive electrode sheet are wound to form a winding core. The winding core is built into the shell. The shell is filled with an electrolyte, and the electrolyte is used to infiltrate the winding core.
[0065] In one embodiment, the negative electrode sheet includes a silicon oxide layer 200, a porous silicon carbon layer 300, a superionic conductor layer 400 and a negative electrode current collector 100, the silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the superionic conductor layer 400 is coated on the porous silicon carbon layer 300; the silicon oxide layer 200 is used to improve the energy density of the negative electrode sheet, the porous silicon carbon layer 300 is used to separate the silicon oxide layer 200 and the superionic conductor, and the superionic conductor layer 400 is used to separate the porous silicon carbon layer 300 and the electrolyte.
[0066] In one embodiment, the superionic conductor layer 400 is composed of a material containing lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3. Lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 can isolate electrons and lithium ions can be easily deintercalated, so that lithium ions can quickly pass through the superionic conductor layer 400 into the porous silicon carbon layer 300. The superionic conductor layer 400 separates the porous silicon carbon layer 300 from the electrolyte, thereby improving the cycle capacity.
[0067] The above-mentioned cylindrical battery for improving the cycle of negative electrode doped silicon power battery and its preparation method, as well as the battery module containing the cylindrical battery, have a higher gram capacity of the silicon oxide layer 200 on the negative electrode sheet, which increases the energy density of the battery. Since the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, that is, the porous silicon carbon layer 300 forms a protective layer on the surface of the silicon oxide layer 200, the silicon oxide layer 200 is blocked from direct contact with the electrolyte, thereby protecting the silicon oxide layer 200 and reducing the expansion of the silicon oxide layer 200 caused by the reaction. Compared with the silicon oxide layer 200, the porous structure of the porous silicon carbon layer 300 is not easy to expand. Furthermore, since the superionic conductor layer 40 is coated on the porous silicon carbon layer 300, the superionic conductor layer 400 separates the porous silicon carbon layer 300 from the electrolyte, reducing the side reaction between the porous silicon carbon layer 300 and the electrolyte, thereby improving the cycle performance and capacity of the battery.
[0068] like Figure 1 As shown, in one embodiment, the number of silicon oxide layers 200, porous silicon carbon layers 300 and super ion conductor layers 400 is two, two silicon oxide layers 200 are respectively coated on both sides of the negative electrode current collector 100, two porous silicon carbon layers 300 are respectively coated on corresponding silicon oxide layers 200, and two super ion conductor layers 400 are respectively coated on corresponding porous silicon carbon layers 300. In this embodiment, coating is performed on both sides of the negative electrode current collector 100, so that the negative electrode current collector 100 can be coated with more silicon oxide layers 200, porous silicon carbon layers 300 and super ion conductor layers 400, thereby effectively improving the battery capacity of the cylindrical battery for improving the cycle of the negative electrode doped silicon power battery.
[0069] like Figure 1 As shown, in one embodiment, the superionic conductor layer 400 is coated by continuous coating, and the thickness of the superionic conductor layer 400 is 1um-2um. In this embodiment, the superionic conductor layer 400 is coated on the surface of the porous silicon carbon layer 300, so that the superionic conductor layer 400 isolates the contact between the electrolyte and the silicon oxide layer 200. The thickness of the superionic conductor layer 400 is relatively thin, so that the thickness of the negative electrode sheet is relatively thin, saving space.
[0070] like Figure 4As shown, the present disclosure also provides a method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery. The cylindrical battery for improving the cycle of a negative electrode doped silicon power battery prepared by the preparation method includes a negative electrode sheet, a positive electrode sheet, a separator and a shell. The negative electrode sheet, the separator and the positive electrode sheet are wound to form a roll core, and the roll core is built into the shell. The shell is also filled with an electrolyte, and the electrolyte is used to infiltrate the roll core; the negative electrode sheet includes a silicon oxide layer 200, a porous silicon carbon layer 300, a superionic conductor layer 400 and a negative electrode current collector 100, the silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the superionic conductor layer 400 is coated on the porous silicon carbon layer 300; the silicon oxide layer 200 is used to improve the energy density of the negative electrode sheet, the porous silicon carbon layer 300 is used to separate the silicon oxide layer 200, and the superionic conductor layer 400 is used to separate the porous silicon carbon layer 300 and the electrolyte.
[0071] Furthermore, the method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery comprises some or all of the following steps:
[0072] S101, the slurry of the silicon oxide layer 200, the slurry of the porous silicon carbon layer 300 and the slurry of the superionic conductor layer 400 are simultaneously coated in multiple layers by a coating device, the slurry of the silicon oxide layer 200 is coated on the negative electrode current collector 100, the slurry of the porous silicon carbon layer 300 is coated on the corresponding slurry surface of the silicon oxide layer 200, and the slurry of the superionic conductor layer 400 is coated on the corresponding slurry surface of the porous silicon carbon layer 300;
[0073] S103, baking the negative electrode current collector 100 coated with the slurry of the silicon oxide layer 200, the slurry of the porous silicon carbon layer 300 and the slurry of the super ion conductor layer 400 at high temperature to form a negative electrode sheet in which the silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the super ion conductor layer 400 is coated on the porous silicon carbon layer 300;
[0074] S105, stacking the negative electrode sheet, the separator and the positive electrode sheet and winding them to form a winding core;
[0075] S107, after flattening and shaping the tabs of the winding core, the winding core is placed in the shell for welding, and the battery cell is obtained after welding;
[0076] S109, a process of injecting liquid into the battery cell;
[0077] S111, welding and sealing the battery cell to obtain a cylindrical battery that improves the cycle of the negative electrode doped silicon power battery.
[0078] It is understandable that if the coating equipment cannot coat the negative electrode current collector 100 at the same time, when the silicon oxide layer 200, the porous silicon carbon layer 300 and the super ion conductor layer 400 are respectively baked at high temperature, it is easier to control the baking time between the silicon oxide layer 200, the porous silicon carbon layer 300 and the super ion conductor layer 400, resulting in the internal silicon oxide layer 200 and the porous silicon carbon layer 300 being easily over-baked. Therefore, the coating equipment needs to perform multi-layer coating on the negative electrode current collector 100 at the same time.
[0079] Furthermore, the coating equipment is provided with a first coating port, a second coating port and a third coating port, the first coating port is used to coat the silicon oxide layer 200, the second coating port is used to coat the porous silicon carbon layer 300, and the third coating port is used to coat the superionic conductor layer 400, the first coating port, the second coating port and the third coating port are successively arranged, and the intervals between the first coating port, the second coating port and the third coating port are 30cm-40cm, and appropriate intervals are set so that the intervals for coating the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 in sequence are short, so that the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor are coated and baked at high temperature at the same time, so that the drying speeds of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor remain consistent.
[0080] The above-mentioned method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery is to coat the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 on the negative electrode current collector 100 in sequence through a coating device, so that the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are dried at the same time, so that the drying speeds of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor 400 are kept consistent, thereby making the bonding strength of the negative electrode current collector 100, the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 better, the porous silicon carbon layer 300 has a better protection effect on the silicon oxide layer 200, and the superionic conductor layer 400 has a better effect of separating the porous silicon carbon layer 300 and the electrolyte, thereby improving the cycle performance of the battery.
[0081] In one embodiment, before winding the positive electrode sheet, the separator and the negative electrode sheet, the following steps are also included:
[0082] A slurry for preparing a silicon oxide layer 200;
[0083] The slurry of the silicon oxide layer 200 includes the following components in various weights:
[0084] Active material graphite Gr: 88.4;
[0085] Silicon dioxide: 8%;
[0086] Polyacrylate lithium PAA-Li: 1.5%;
[0087] Sodium carboxymethyl cellulose CMC2200: 0.5%;
[0088] Conductive carbon black SP: 0.5%;
[0089] Single-walled carbon tubes SWCNTs: 0.4%;
[0090] Styrene butadiene rubber emulsion SBR: 0.7%;
[0091] In one embodiment, the process of making silicon monoxide further comprises the following steps:
[0092] Alkali metal silicate is mixed with an inorganic acidic solvent to obtain a hydrosol of silica, and then gel particles of silica are formed through the control of colloid particles; the gel particles of silica are dried, cleaned, and then dried to form gel particles with high purity; silica is calcined to obtain silica; silica and elemental silicon are mixed, and heated under a negative pressure environment for disproportionation reaction to obtain silicon dioxide; silicon dioxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tubes SWCNTs and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring, and then the stirred silicon dioxide layer 200 is stored in a transfer tank, and the transfer tank of the silicon dioxide layer 200 is connected to the first coating port of the coating device.
[0093] Furthermore, the lithium polyacrylate PAA-Li in the silicon oxide layer 200 is a lithium salt. Compared with sodium polyacrylate PAA-Na, lithium polyacrylate PAA-Li increases the lithium ion deintercalation space, improves the lithium ion conductivity of the surface coating of the silicon oxide layer 200, and thus improves the low-temperature discharge performance. In addition, since lithium polyacrylate PAA-Li contains more carboxyl groups, the abundant carboxyl groups form hydrogen bonds with silicon particles, increasing the binding force between silicon particles and the current collector, so that lithium polyacrylate PAA-Li has the thickening effect of sodium carboxymethyl cellulose CMC2200 and the bonding effect of styrene butadiene rubber emulsion SBR, thereby reducing the use of lithium carboxymethyl cellulose sodium CMC2200 and styrene butadiene rubber emulsion SBR. Compared with carbon black, single-walled carbon tubes SWCNTs can form a line contact and surface contact conductive network between active substances, thereby improving the conductive performance and reducing impedance.
[0094] In one embodiment, before the positive electrode sheet, the separator and the negative electrode sheet are wound, after the slurry for making the porous silicon carbon layer 300 is coated on the negative electrode current collector 100, the following steps are also included:
[0095] A slurry for making a porous silicon carbon layer 300;
[0096] Slurry of the porous silicon carbon layer 300 The porous silicon carbon layer 300 includes the following components in various qualities:
[0097] Active material graphite Gr: 87.1%;
[0098] Porous silicon carbon: 10%;
[0099] Polyacrylate lithium PAA-Li: 1.5%;
[0100] Sodium carboxymethyl cellulose CMC2200: 0.5%;
[0101] Single-walled carbon tubes SWCNTs: 0.4%;
[0102] Styrene butadiene rubber emulsion SBR: 0.7%;
[0103] In one embodiment, the slurry of the porous silicon carbon layer 300 is coated on the surface of the slurry of the silicon oxide layer 200. In this embodiment, the preparation of the porous silicon carbon layer 300 includes the following steps:
[0104] First, the carbon material is subjected to high temperature treatment to form a porous conductive carbon material with multiple pores; an inert gas is introduced into the porous conductive carbon material under a high temperature environment; and a gas containing silicon components is introduced into the porous conductive carbon material for vapor deposition to obtain porous silicon carbon. The porous silicon carbon layer 300 is then placed in a stirring tank with polyacrylate lithium PAA-Li, carboxymethyl cellulose sodium CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR for mixing and stirring, and then the stirred porous silicon carbon layer 300 is stored in a transfer tank, and the transfer tank of the porous silicon carbon layer 300 is connected to the second coating port of the coating device.
[0105] Furthermore, the porous silicon carbon uses porous carbon as a skeleton, and silicon nanoparticles are dispersed in the pores of the porous conductive carbon material by vapor deposition. The pores provide a buffer space for the silicon particles during the charging and discharging process, making the porous silicon carbon layer 300 less likely to expand, and also provide a channel for the transmission of lithium ions, thereby improving the electrochemical performance and stability of the porous silicon carbon layer 300.
[0106] It can be understood that the lithium polyacrylate PAA-Li in the porous silicon carbon layer 300 is a lithium salt. Compared with sodium polyacrylate PAA-Na, lithium polyacrylate PAA-Li increases the deintercalation space of lithium ions, improves the conductivity of lithium ions coated on the surface of the porous silicon carbon layer 300, and thus improves the low-temperature discharge performance of the battery.
[0107] In one of the embodiments, when the slurry of the porous silicon carbon layer 300 and the slurry of the silicon oxide layer 200 are coated on the negative electrode current collector and baked at high temperature, the internal solvent of the slurry of the porous silicon carbon layer 300 and the slurry of the silicon oxide layer 200 will evaporate, and the solvent will evaporate from the silicon oxide layer 200 coating to the porous silicon carbon layer 300 coating. The solvent flow process will bring the conductive carbon black SP and single-walled carbon tubes SWCNTs with smaller particle sizes to the porous silicon carbon layer 300 coating and the superionic conductor layer 400. The conductive carbon black SP and the single-walled carbon tubes SWCNTs have a small specific surface area, and the conductive carbon black SP and the single-walled carbon tubes SWCNTs are easy to produce side reactions with the electrolyte on the surface of the superionic conductor layer 400. When the porous silicon carbon layer 300 is prepared, the amount of single-walled carbon tubes SWCNTs or conductive carbon black SP is reduced. When the superionic conductor layer 400 is prepared, the superionic conductor layer 400 does not contain single-walled carbon tubes SWCNTs or conductive carbon black SP, so that the amount of single-walled carbon tubes SWCNTs or conductive carbon black SP decreases gradually from the inside to the outside. The single-walled carbon tubes SWCNTs or conductive carbon black SP enter the porous silicon carbon layer 300 and the superionic conductor layer 400 in turn, and part of the single-walled carbon tubes SWCNTs or conductive carbon black SP stays in the porous silicon carbon layer 300, reducing the amount of single-walled carbon tubes SWCNTs or conductive carbon black SP floating from the silicon oxide layer 200 and the porous silicon carbon layer 300 to the superionic conductor layer 400 with the solvent, thereby reducing the side reactions of the conductive carbon black SP and the single-walled carbon tubes SWCNTs with the electrolyte on the surface of the superionic conductor layer 400, thereby improving the cycle performance of the battery.
[0108] In one embodiment, before the positive electrode sheet, the separator and the negative electrode sheet are wound, the slurry for making the porous silicon carbon layer 300 is coated on the slurry of the porous silicon carbon layer 300, and the following steps are also included:
[0109] First, a slurry for the super ion conductor layer 400 is prepared. Lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 is a good conductor of lithium ions and an insulator of electrons.
[0110] In one embodiment, the slurry of the superionic conductor layer 400 includes the following components in respective weights:
[0111] Lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6 (PO4) 3: 96%;
[0112] Adhesive: 2.5%;
[0113] Styrene butadiene rubber emulsion SBR: 1.5%;
[0114] Then, the slurry of the super ion conductor layer 400 is coated on the surface of the slurry of the silicon oxide layer 200 .
[0115] Furthermore, the preparation of lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 includes the following steps:
[0116] First, lithium carbonate, alumina ceramics, titanium dioxide, and ammonium dihydrogen phosphate are mixed in a certain proportion; the mixture of lithium carbonate, alumina ceramics, titanium dioxide, and ammonium dihydrogen phosphate is heated to 900-1000°C in a reducing atmosphere of carbon monoxide to obtain lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3; the lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 is then put into a stirring tank with an adhesive and styrene-butadiene rubber emulsion SBR for mixing and stirring to form a superionic conductor layer 400; the stirred superionic conductor layer 400 is then stored in a transfer tank, and the transfer tank of the superionic conductor layer 400 is connected to the third coating port of the coating device.
[0117] In this embodiment, lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6 (PO4) 3 acts as a good conductor of lithium ions and an insulator of electrons. When the temperature decreases, the viscosity of the electrolyte increases, while the temperature has little effect on the lithium ion conductivity of lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6 (PO4) 3, so that lithium ions can be quickly exchanged in the superionic conductor layer 400 under low temperature conditions, thereby improving the low-temperature discharge performance of the cylindrical battery of the negative electrode doped silicon power battery cycle.
[0118] However, during the multi-layer coating process, the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are mutually soluble due to different surface tensions. In one embodiment, by controlling the surface tension between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, that is, controlling the addition of the same proportion of adhesive such as polyacrylate lithium PAA-Li to the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, the effect of the adhesive on the surface tension between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is reduced.
[0119] Furthermore, when preparing the silicon oxide layer 200, firstly, silicon oxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring; then, before the stirred silicon oxide layer 200 is stored in a transfer tank, the viscosity value of the silicon oxide layer 200 is tested; then, when preparing the porous silicon carbon layer 300, the porous silicon carbon layer 300, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring; then, the stirred porous silicon Before the carbon layer 300 is stored in the transfer tank; then the solid content of the porous silicon carbon layer 300 is adjusted according to the viscosity value of the silicon oxide layer 200, so that the viscosity value of the porous silicon carbon layer 300 is close to the viscosity value of the silicon oxide layer 200; then when making the superionic conductor layer 400, lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3, adhesive, and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring to make the superionic conductor layer 400, and after the stirred superionic conductor layer 400 passes through the transfer tank, the solid content of the superionic conductor layer 400 is adjusted according to the viscosity value of the porous silicon carbon layer 300, so that the viscosity value of the superionic conductor layer 400 is close to the viscosity value of the porous silicon carbon layer 300. Since the viscosity value has a certain influence on the surface tension between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, the viscosity values of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are adjusted to be similar, thereby reducing the influence of the surface tension between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, thereby reducing the mutual solubility between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, making the stratification between the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 more obvious.
[0120] Furthermore, when the viscosity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor 400 is too high, the fluidity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is poor, which is not conducive to the leveling of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, so that the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are coated. When the viscosity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor 400 is too low, the fluidity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is good, but the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are difficult to dry. Therefore, it is necessary to control the viscosity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor 400 within 3000Pa.s-6000Pa.s, so that the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor 400 have certain fluidity when coated and dry quickly.
[0121] However, in the multi-layer coating process, the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 need to be added into the corresponding slurry for stirring; then the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are mixed with the mixture of the slurry respectively; and then coating is performed; because the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 will evaporate the solvent during the high-temperature drying process, the solvent evaporation speed is too fast, which can easily cause the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 to be mutually soluble. Furthermore, when preparing the silicon oxide layer 200, when silicon oxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR are placed in a stirring tank for mixing and stirring, the mixed slurry is added for mixing, thereby increasing the proportion of the silicon oxide layer 200 in the slurry and increasing the solid content of the silicon oxide layer 200 in the slurry mixture; when preparing the porous silicon carbon layer 300, the porous silicon carbon layer 300, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR are placed in a stirring tank for mixing and stirring, and the mixed slurry is added for mixing, thereby increasing the proportion of the silicon oxide layer 200 in the slurry and increasing the solid content of the silicon oxide layer 200 in the slurry mixture. When SP, single-walled carbon tubes SWCNTs and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring, the slurry is added for mixing, thereby increasing the solid content of the porous silicon carbon layer 300 in the slurry mixture; when the superionic conductor layer 400 is made, lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6 (PO4) 3 is put into a stirring tank for mixing and stirring with an adhesive and styrene-butadiene rubber emulsion SBR to make the superionic conductor layer 400, and the slurry is added for mixing, thereby increasing the proportion of the superionic conductor layer 400 in the slurry, thereby increasing the solid content of the superionic conductor layer 400 in the slurry mixture. The solid content of the slurry mixture of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is controlled between 40% and 55%. The increased solid content of the slurry mixture of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 shortens the stirring time and consumes less solvent, thereby reducing the volatilization of the solvent and improving the mutual solubility among the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400.
[0122] In one embodiment, the mass capacity ratio of the porous silicon carbon layer 300 to the silicon oxide layer 200 is 0.05-0.25. In this embodiment, the gram capacity of silicon oxide 200 is higher than the gram capacity of the porous silicon carbon 300, so when better cycle performance is required, the silicon oxide layer 200 is thicker than the porous silicon carbon layer 300, so that the gram capacity of the negative electrode sheet is higher, and the porous silicon carbon layer 300 needs to have a certain thickness so that the porous silicon carbon layer 300 has a better effect of isolating the silicon oxide layer 200. In turn, the mass capacity ratio of the porous silicon carbon layer 300 to the silicon oxide layer 200 needs to be controlled at an appropriate ratio according to the number of cycles.
[0123] Furthermore, during the coating process, the first coating port, the second coating port, and the third coating port coat different amounts of the silicon monoxide layer 200, the porous silicon carbon layer 300, and the super ionic conductor layer 400, respectively. It is necessary to control the first coating port, the second coating port and the third coating port of the coating equipment for debugging respectively. The coating device controls the output thickness by controlling the size of the output port. The coating device controls the pressure of the output material and the flow rate of the output slurry by controlling the mass capacity ratio of the porous silicon carbon layer 300, the silicon oxide layer 200 and the superionic conductor layer 400. During coating, the temperature of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is controlled between 15°C and 35°C to enable the coating device to discharge the material smoothly; place the empty foil at the first coating port for coating, and adjust the surface density of the silicon oxide layer 200 coated at the first coating port; then place the empty foil at the second coating port, and adjust the surface density of the porous silicon carbon layer 300 coated at the second coating port; then place the empty foil at the third coating port, and adjust the third coating port to coat the superionic conductor layer 400. When a specific mass capacity ratio of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is required, the discharge of the silicon oxide layer 200 from the first coating port, the discharge of the porous silicon carbon layer 300 from the second coating port and the discharge of the superionic conductor layer 400 from the third coating port are adjusted in the coater respectively, so that the coater can accurately coat the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 in sequence on the negative electrode current collector 100 according to the set ratio, thereby realizing batch continuous coating production and improving the production efficiency of the negative electrode sheets.
[0124] Since the viscosity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 gradually decreases, the stability of the hierarchical structure of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 before drying and curing is poor. Further, the cross-sections of the first coating port, the second coating port and the third coating port gradually decrease, and the extrusion amount of the first coating port, the second coating port and the third coating port per unit time is adapted to the difference in layer thickness to adapt to the problem of the gradually decreasing viscosity of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400, thereby solving the problem of the poor stability of the hierarchical structure of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 before drying and curing. Specifically, the width of the cross-sections of the first coating port, the second coating port and the third coating port gradually decreases.
[0125] Furthermore, the extrusion pressure of the first coating port, the second coating port and the third coating port is gradually reduced, so that the thickness of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 becomes thinner and thinner, which better adapts to the viscosity difference of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400.
[0126] Furthermore, the distance between the first coating port and the empty foil is a first distance, the distance between the second coating port and the empty foil is a second distance, and the distance between the third coating port and the empty foil is a third distance; the first distance is greater than the second distance, and the second distance is greater than the third distance, so that the thickness of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 of the electrode can be formed more smoothly and orderly, less prone to interference, and better adapted to the gradually decreasing differences in cross-sections of the first coating port, the second coating port and the third coating port.
[0127] In one embodiment, the binder includes lithium carboxymethyl cellulose CMC-Li and lithium polyacrylate PAA-Li. In this embodiment, the binder lithium carboxymethyl cellulose CMC-Li and lithium polyacrylate PAA-Li with ion conductivity further improves the ion conductivity and the exchange rate of lithium ions, thereby improving the cycle performance of the cylindrical battery with negative electrode doped silicon power battery cycle.
[0128] The present disclosure also provides a battery module for cylindrical batteries for improving the cycle of negative electrode silicon-doped power batteries, including any of the above-mentioned cylindrical batteries for improving the cycle of negative electrode silicon-doped power batteries. The cylindrical battery for improving the cycle of negative electrode silicon-doped power batteries includes a negative electrode sheet, a positive electrode sheet, a diaphragm and a shell. The negative electrode sheet, the diaphragm and the positive electrode sheet are wound to form a core, and the core is built into the shell. The shell is also filled with electrolyte, and the electrolyte is used to infiltrate the core. The negative electrode sheet includes a silicon oxide layer 200, a porous silicon carbon layer 300, a superionic conductor layer 400 and a negative electrode current collector 100, the silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the superionic conductor layer 400 is coated on the porous silicon carbon layer 300; the silicon oxide layer 200 is used to improve the energy density of the negative electrode sheet, the porous silicon carbon layer 300 is used to separate the silicon oxide layer 200 and the superionic conductor, and the superionic conductor layer 400 is used to separate the porous silicon carbon layer 300 and the electrolyte. In this embodiment, the gram capacity of the silicon oxide layer 200 on the negative electrode sheet is relatively high, which increases the energy density of the battery. The porous silicon carbon layer 300 forms a protective layer on the surface of the silicon oxide layer 200, blocking the silicon oxide layer 200 from contacting the electrolyte, protecting the silicon oxide layer 200, and reducing the expansion of the silicon oxide layer 200 caused by the reaction. The porous structure of the porous silicon carbon layer 300 is not easy to expand. The superionic conductor layer 400 separates the porous silicon carbon layer 300 from the electrolyte, avoiding side reactions between the porous silicon carbon layer 300 and the electrolyte, thereby improving the cycle performance and capacity of the battery module of the cylindrical battery that improves the cycle of the negative electrode doped silicon power battery.
[0129] Compared with the prior art, the present invention has the following advantages, including but not limited to:
[0130] 1. The cylindrical battery for improving the cycle of negative electrode doped silicon power battery and its preparation method, as well as the battery module containing the cylindrical battery, have a high gram capacity of the silicon oxide layer 200 on the negative electrode sheet, which increases the energy density of the battery. Since the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, that is, the porous silicon carbon layer 300 forms a protective layer on the surface of the silicon oxide layer 200, the silicon oxide layer 200 is blocked from direct contact with the electrolyte, thereby protecting the silicon oxide layer 200 and reducing the expansion of the silicon oxide layer 200 caused by the reaction. Compared with the silicon oxide layer 200, the porous structure of the porous silicon carbon layer 300 is not easy to expand. Furthermore, since the superionic conductor layer 40 is coated on the porous silicon carbon layer 300, the superionic conductor layer 400 separates the porous silicon carbon layer 300 from the electrolyte, reducing the side reaction between the porous silicon carbon layer 300 and the electrolyte, thereby improving the cycle performance and capacity of the battery.
[0131] 2. The silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 are coated on the negative electrode current collector 100 from the inside to the outside in sequence by means of a coating device, and during the preparation, the slurry of the silicon oxide layer 200, the slurry of the porous silicon carbon layer 300 and the slurry of the superionic conductor layer 400 are dried at the same time, so that the drying speeds of the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor are kept almost the same, so that the negative electrode current collector 100, the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 have better bonding strength, the porous silicon carbon layer 300 has a better protection effect on the silicon oxide layer 200, and the superionic conductor layer 400 has a better effect of separating the porous silicon carbon layer 300 and the electrolyte, thereby improving the cycle performance of the battery.
[0132] 3. By using adhesives such as lithium carboxymethyl cellulose CMC-Li and lithium polyacrylate PAA-Li, compared with traditional sodium salt adhesives, the permeability of lithium ions in the silicon oxide layer 200, the porous silicon carbon layer 300, and the superionic conductor layer 400 is increased, thereby improving the discharge performance of the cylindrical battery of the negative electrode doped silicon power battery cycle.
[0133] Some specific examples are listed below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.
[0134] For the silicon oxide layer 200, the active material graphite Gr. is 88.4 kg, silicon oxide is 8 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene butadiene rubber latex SBR is 0.7 kg; for the porous silicon carbon layer 300, the active material graphite Gr. is 86.4 kg, porous silicon carbon is 10 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene butadiene rubber latex SBR is 0.7 kg;
[0135] The silicon oxide layer 200 is coated on the negative electrode current collector 100, and the porous silicon carbon layer 300 is coated on the silicon oxide layer 200. The negative electrode current collector 100 coated with the silicon oxide layer 200 and the porous silicon carbon layer 300 is baked at high temperature to form a negative electrode sheet. The negative electrode sheet, the separator and the positive electrode sheet are stacked and then wound to form a battery cell. After the tabs of the battery cell are flattened and shaped, the battery cell is placed in a shell and welded. After welding, a liquid injection process is performed. The battery cell is welded and sealed to form a cylindrical battery for improving the cycle of the negative electrode doped silicon power battery of Example 1.
[0136] For the silicon oxide layer 200, the active material graphite Gr. is 88.4 kg, silicon oxide is 8 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene-butadiene rubber latex SBR is 0.7 kg; for the porous silicon carbon layer 300, the active material graphite Gr. is 87.1 kg, porous silicon carbon is 10 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.2 kg, conductive carbon black SP is 0.2 kg, single-walled carbon tube is 0.7 kg, and styrene-butadiene rubber latex SBR is 0.7 kg;
[0137] The silicon oxide layer 200 is coated on the negative electrode current collector 100, and the porous silicon carbon layer 300 is coated on the silicon oxide layer 200. The negative electrode current collector 100 coated with the silicon oxide layer 200 and the porous silicon carbon layer 300 is baked at high temperature to form a negative electrode sheet. The negative electrode sheet, the separator and the positive electrode sheet are stacked and wound to form a battery cell. After the tabs of the battery cell are flattened and shaped, the battery cell is placed in a shell and welded. After welding, a liquid injection forming process is performed. The battery cell is welded and sealed to form a cylindrical battery for improving the cycle of the negative electrode doped silicon power battery of Example 2.
[0138] For the silicon oxide layer 200, the active material graphite Gr. is 88.4 kg, silicon oxide is 8 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene-butadiene rubber latex SBR is 0.7 kg; for the porous silicon carbon layer 300, the active material graphite Gr. is 87.1 kg, porous silicon carbon is 10 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene-butadiene rubber latex SBR is 0.7 kg. The superionic conductor layer 400 is composed of 96kg of lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3, 1.5kg of sodium polyacrylate PAA-Na, 1.5kg of styrene butadiene rubber emulsion SBR, and 1kg of sodium carboxymethyl cellulose CMC2200;
[0139] The silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the superionic conductor layer 400 is coated on the porous silicon carbon layer 300. The negative electrode current collector 100 coated with the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is baked at a high temperature to form a negative electrode sheet. The negative electrode sheet, the separator and the positive electrode sheet are stacked and wound to form a battery cell. After the tabs of the battery cell are flattened and shaped, the battery cell is placed in a shell and welded. After welding, a liquid injection forming process is performed. The battery cell is welded and sealed to form a cylindrical battery for improving the cycle of the negative electrode doped silicon power battery of Example 3.
[0140] For the silicon oxide layer 200, the active material graphite Gr. is 88.4 kg, silicon oxide is 8 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene-butadiene rubber latex SBR is 0.7 kg; for the porous silicon carbon layer 300, the active material graphite Gr. is 87.1 kg, porous silicon carbon is 10 kg, polyacrylate lithium PAA-Li is 1.5 kg, sodium carboxymethyl cellulose CMC2200 is 0.5 kg, conductive carbon black SP is 0.5 kg, single-walled carbon tube is 0.4 kg, and styrene-butadiene rubber latex SBR is 0.7 kg. The weight of the superionic conductor layer 400 is 1.5kg, the weight of sodium carboxymethyl cellulose CMC2200 is 0.5kg, the weight of conductive carbon black SP is 0.2kg, the weight of single-walled carbon tube is 0.7kg, and the weight of styrene-butadiene rubber emulsion SBR is 0.7kg; for the superionic conductor layer 400, the weight of lithium aluminum titanium phosphate Li1.4AlO.4Ti1.6(PO4)3 is 96kg, the weight of lithium polyacrylate PAA-Li is 1.5kg, the weight of styrene-butadiene rubber emulsion SBR is 1.5kg, and the weight of lithium carboxymethyl cellulose CMC-Li is 1kg;
[0141] The silicon oxide layer 200 is coated on the negative electrode current collector 100, the porous silicon carbon layer 300 is coated on the silicon oxide layer 200, and the superionic conductor layer 400 is coated on the porous silicon carbon layer 300. The negative electrode current collector 100 coated with the silicon oxide layer 200, the porous silicon carbon layer 300 and the superionic conductor layer 400 is baked at a high temperature to form a negative electrode sheet. The negative electrode sheet, the separator and the positive electrode sheet are stacked and wound to form a battery cell. After the tabs of the battery cell are flattened and shaped, the battery cell is placed in a shell and welded. After welding, a liquid injection forming process is performed. The battery cell is welded and sealed to form a cylindrical battery for improving the cycle of the negative electrode doped silicon power battery of Example 3.
[0142] Comparative Example 1
[0143] The silicon oxide layer 200 is composed of 88.4 kg of active graphite Gr., 8 kg of silicon oxide, 1.5 kg of lithium polyacrylate PAA-Li, 0.5 kg of sodium carboxymethyl cellulose CMC2200, 0.5 kg of conductive carbon black SP, 0.4 kg of single-walled carbon tube, and 0.7 kg of styrene-butadiene rubber latex SBR;
[0144] The silicon oxide layer 200 is coated on the negative electrode current collector 100, and the negative electrode current collector 100 coated with the silicon oxide layer 200 is baked at high temperature to form a negative electrode sheet. The negative electrode sheet, the separator and the positive electrode sheet are stacked and then wound to form a battery cell; after the tabs of the battery cell are flattened and shaped, the battery cell is placed in a shell and welded, and after welding, a liquid injection process is performed; the battery cell is welded and sealed to form a cylindrical battery for improving the cycle of the negative electrode doped silicon power battery of comparative example 1.
[0145] Figure 5 The figure shows the comparison of the retention rate of the 300cls cycle capacity at 45°C and 55°C for Comparative Example 1, Example 1, Example 2, Example 3 and Example 4, respectively. Compared with Example 1, Example 1 using the porous silicon carbon layer 300 reduces the capacity decay of the cycle; Compared with Example 1, Example 2 has less conductive carbon black SP and single-walled carbon tubes SWCNTs in the porous silicon carbon layer 300, and Example 2 reduces the cycle capacity decay; Compared with Example 2, Example 3, in which the porous silicon carbon layer 300 is coated with a superionic conductor layer 400, can reduce the cycle capacity decay; Compared with Example 3, Example 4, in which the adhesive uses carboxymethyl cellulose lithium CMC-Li and polyacrylic acid lithium PAA-Li, has the best effect in reducing the cycle capacity decay.
[0146] Figure 6The figure shows the comparison of the negative electrode thickness expansion rate of Comparative Example 1, Example 1, Example 2, Example 3 and Example 4 at 45°C and 55°C respectively. Compared with Example 1, Comparative Example 1 reduces the negative electrode thickness expansion of Example 1 using the porous silicon carbon layer 300; compared with Comparative Example 1, Example 3 and Example 4 use the porous silicon carbon layer 300 coated with the silicon oxide layer, and the super ion conductor layer 400 coated with the porous silicon carbon layer 300, and the negative electrode thickness expansion rate of Example 3 and Example 4 is lower.
[0147] Figure 7 The figures show the residual capacity of Comparative Example 1, Example 1, Example 2, Example 3 and Example 4 after 7 days of storage at 60°C. Compared with Comparative Example 1, the residual capacity of Examples 3 and 4 after 7 days of storage at 60°C, which use the porous silicon carbon layer 300 to coat the silicon oxide layer and the superionic conductor layer 400 to coat the porous silicon carbon layer 300, is higher.
[0148] Figure 8 The figure shows the comparison of the discharge at -20°C 1C of Comparative Example 1, Example 1, Example 2, Example 3 and Example 4. Compared with Comparative Example 1, Example 3 and Example 4 use a porous silicon carbon layer 300 to coat the silicon oxide layer, and a superionic conductor layer 400 to coat the porous silicon carbon layer 300, and the discharge speed at -20°C 1C of Example 3 and Example 4 is faster.
[0149] Combination Figures 6 to 8 , and obtain the data in Table 1 below:
[0150]
[0151] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the disclosed patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the disclosed patent shall be subject to the attached claims.
Claims
1. A method for preparing a cylindrical battery for improving the cycle of a negative electrode doped with silicon power battery, characterized in that: Used to prepare a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery, the cylindrical battery for improving the cycle of a negative electrode doped silicon power battery comprises a negative electrode sheet, a positive electrode sheet, a separator and a shell, the negative electrode sheet, the separator and the positive electrode sheet are wound to form a roll core, the roll core is built into the shell, the shell is also filled with an electrolyte, the electrolyte is used to infiltrate the roll core; the negative electrode sheet comprises a silicon oxide layer, a porous silicon carbon layer, a superionic conductor layer and a negative electrode current collector, the silicon oxide layer is coated on the negative electrode current collector, the porous silicon carbon layer is coated on the silicon oxide layer, the superionic conductor layer is coated on the porous silicon carbon layer; the porous silicon The carbon layer is used to separate the silicon oxide layer and the superionic conductor layer, and the superionic conductor layer is used to separate the porous silicon carbon layer and the electrolyte; the number of the silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer is two, the two silicon oxide layers are respectively coated on both sides of the negative electrode current collector, the two porous silicon carbon layers are respectively coated on the corresponding silicon oxide layers, and the two superionic conductor layers are respectively coated on the corresponding porous silicon carbon layers; the superionic conductor layer is coated by continuous coating, and the thickness of the superionic conductor layer is 1μm-2μm; the preparation method comprises the following steps: a slurry for making a silicon oxide layer; The slurry of silicon dioxide layer includes the following components in different weights: Active material graphite Gr: 88.4%; Silicon dioxide: 8%; Polyacrylate lithium PAA-Li: 1.5%; Sodium carboxymethyl cellulose CMC2200: 0.5%; Conductive carbon black SP: 0.5%; Single-walled carbon tubes SWCNTs: 0.4%; Styrene butadiene rubber emulsion SBR: 0.7%; Put silicon dioxide, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tube SWCNTs and styrene-butadiene rubber emulsion SBR into a stirring tank for mixing and stirring, then store the stirred silicon dioxide layer slurry through a transfer tank, the transfer tank of the silicon dioxide layer slurry is connected to the first coating port of the coating device; then test the viscosity value of the silicon dioxide layer slurry before storing the stirred silicon dioxide layer slurry through the transfer tank; a slurry for making a porous silicon carbon layer; The slurry of the porous silicon carbon layer includes the following components in various weights: Active material graphite Gr: 87.1kg; Porous silicon carbon: 10kg; Polyacrylate lithium PAA-Li: 1.5kg; Sodium carboxymethyl cellulose CMC2200: 0.5kg; Conductive carbon black SP: 0.2kg; Single-walled carbon tubes SWCNTs: 0.7kg; Styrene butadiene rubber emulsion SBR: 0.7kg; Porous silicon carbon, lithium polyacrylate PAA-Li, sodium carboxymethyl cellulose CMC2200, conductive carbon black SP, single-walled carbon tubes SWCNTs and styrene-butadiene rubber emulsion SBR are placed in a stirring tank for mixing and stirring, and then the stirred slurry of the porous silicon carbon layer is stored through a transfer tank, and the transfer tank of the slurry of the porous silicon carbon layer is connected to the second coating port of the coating device; then the stirred slurry of the porous silicon carbon layer is stored through the transfer tank; and then the solid content of the slurry of the porous silicon carbon layer is adjusted according to the viscosity value of the slurry of the silicon oxide layer, so that the viscosity value of the slurry of the porous silicon carbon layer is close to the viscosity value of the slurry of the silicon oxide layer; The slurry of the superionic conductor layer is prepared, and the slurry of the superionic conductor layer includes the following components in various weights: Lithium Aluminum Titanium Phosphate 1.4 Al 0.4 Ti 1.6 (PO4) 3: 96%; Adhesive: 2.5%; Styrene butadiene rubber emulsion SBR: 1.5%; The adhesive comprises lithium polyacrylate PAA-Li and lithium carboxymethyl cellulose CMC-Li, and the mass ratio of the lithium polyacrylate PAA-Li to the lithium carboxymethyl cellulose CMC-Li is 1.5:1; Lithium Aluminum Titanate Phosphate 1.4 Al 0.4 Ti 1.6 (PO4)3, an adhesive and styrene-butadiene rubber emulsion SBR are put into a stirring tank for mixing and stirring to form a slurry of a superionic conductor layer, and then the stirred slurry of the superionic conductor layer is stored through a transfer tank, and the transfer tank of the slurry of the superionic conductor layer is connected to the third coating port of the coating device. After the stirred slurry of the superionic conductor layer passes through the transfer tank, the solid content of the slurry of the superionic conductor layer is adjusted according to the viscosity value of the slurry of the porous silicon carbon layer, so that the viscosity value of the slurry of the superionic conductor layer is close to the viscosity value of the slurry of the porous silicon carbon layer, and the viscosity values of the slurry of the silicon oxide layer, the slurry of the porous silicon carbon layer and the slurry of the superionic conductor layer are controlled within 3000Pa.s-6000Pa.s; The solid content of the slurry mixture of the silicon oxide layer, the porous silicon carbon layer and the superionic conductor layer is controlled between 40% and 55%; The slurry of the silicon oxide layer, the slurry of the porous silicon carbon layer and the slurry of the superionic conductor layer are simultaneously coated in multiple layers by a coating device, the slurry of the silicon oxide layer is coated on the negative electrode current collector, the slurry of the porous silicon carbon layer is coated on the corresponding slurry surface of the silicon oxide layer, and the slurry of the superionic conductor layer is coated on the corresponding slurry surface of the porous silicon carbon layer; the capacity ratio of the porous silicon carbon layer to the silicon oxide layer is 0.05-0.25; The coating equipment is provided with a first coating port, a second coating port and a third coating port, the first coating port is used for coating a silicon oxide layer, the second coating port is used for coating a porous silicon carbon layer, and the third coating port is used for coating a superionic conductor layer. The first coating port, the second coating port and the third coating port are arranged in sequence, and the interval between the first coating port, the second coating port and the third coating port is 30 cm-40 cm; During the coating process, the first coating port, the second coating port and the third coating port respectively coat different amounts of silicon dioxide layer, porous silicon carbon layer and superionic conductor layer; it is necessary to control the first coating port, the second coating port and the third coating port of the coating equipment to be debugged respectively, the coating device controls the output thickness by controlling the size of the output port, and the coating device controls the pressure of the output material and the flow rate of the output slurry by controlling the mass capacity ratio of the porous silicon carbon layer, the silicon dioxide layer and the superionic conductor layer. During coating, the temperature of the silicon dioxide layer, the porous silicon carbon layer and the superionic conductor layer is controlled between 15°C and 35°C to enable the coating device to discharge materials smoothly; the empty foil is placed at the first coating port for coating, and the surface density of the silicon dioxide layer coated at the first coating port is adjusted; the empty foil is then placed at the second coating port, and the surface density of the porous silicon carbon layer coated at the second coating port is adjusted; the empty foil is then placed at the third coating port, and the third coating port is adjusted to coat the superionic conductor layer; The cross sections of the first coating port, the second coating port and the third coating port are gradually reduced, and the extrusion pressure of the first coating port, the second coating port and the third coating port is gradually reduced; The distance between the first coating port and the empty foil is a first distance, the distance between the second coating port and the empty foil is a second distance, and the distance between the third coating port and the empty foil is a third distance; the first distance is greater than the second distance, and the second distance is greater than the third distance; The negative electrode current collector coated with the slurry of the silicon oxide layer, the slurry of the porous silicon carbon layer and the slurry of the super ion conductor layer is baked at high temperature to form the negative electrode sheet in which the silicon oxide layer is coated on the negative electrode current collector, the porous silicon carbon layer is coated on the silicon oxide layer, and the super ion conductor layer is coated on the porous silicon carbon layer; The negative electrode sheet, the separator and the positive electrode sheet are stacked and then wound to form the winding core; After flattening and shaping the tabs of the winding core, the winding core is placed in the shell for welding, and a battery cell is obtained after welding; The battery cell is subjected to a process of injecting liquid into the battery cell; The battery core is welded and sealed to obtain the cylindrical battery for improving the cycle of the negative electrode doped silicon power battery.
2. A battery module, characterized in that: A cylindrical battery for improving the cycle of a negative electrode doped silicon power battery prepared by the method for preparing a cylindrical battery for improving the cycle of a negative electrode doped silicon power battery as described in claim 1.