Tantalum carbide slurry, tantalum carbide coating, preparation method thereof and crucible

By coating the surface of tantalum carbide powder with a polymer resin layer and adding appropriate amounts of sintering aids, binders and solvents, the problems of cracking and density inhomogeneity of tantalum carbide coatings during powder sintering were solved, and a high-density, low-crack tantalum carbide coating was prepared, which improved the stability and uniformity of the crucible.

CN118063214BActive Publication Date: 2024-11-12HUNAN KAIXIN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410076262.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-18
Publication Date
2024-11-12
Estimated Expiration
2044-01-18

AI Technical Summary

Technical Problem

Existing tantalum carbide coatings are prone to cracking and density inhomogeneity during powder sintering, resulting in low coating density. Furthermore, tantalum carbide powder is prone to sedimentation and agglomeration, affecting the stability and uniformity of the crucible.

Method used

By coating the surface of tantalum carbide powder with a polymer resin layer to form a modified tantalum carbide slurry, and combining it with appropriate amounts of sintering aids, binders and solvents, a tantalum carbide coating with high stability and high carbon content is prepared, which controls the shrinkage rate and thermal stress during the sintering process and prevents cracking.

Benefits of technology

A high-density, low-crack tantalum carbide coating was achieved, which improved the uniformity and stability of the crucible and enhanced its service life and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118063214B_ABST
    Figure CN118063214B_ABST
Patent Text Reader

Abstract

The present invention relates to a tantalum carbide slurry, a tantalum carbide coating, a preparation method thereof and a crucible. The tantalum carbide slurry comprises, by weight, 70 to 80 parts of modified tantalum carbide, 0.5 to 1.0 parts of a sintering aid, 0.5 to 1.0 parts of a binder and 18.5 to 28 parts of a solvent; the modified tantalum carbide comprises tantalum carbide and a polymer resin layer, and the polymer resin layer is coated on the surface of the tantalum carbide. The above-mentioned tantalum carbide slurry is formed by matching the components according to a specific ratio to form a slurry with good stability, high tantalum carbide content, and the ability to form a coating layer with a high stacking density; the slurry can form a tantalum carbide coating with a high carbon content, high density and few cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crucibles, and in particular to a tantalum carbide slurry, a tantalum carbide coating and a preparation method thereof, and a crucible. Background Art

[0002] Tantalum carbide is an ideal substrate material for crucibles used for single crystal growth due to its excellent thermal stability and chemical inertness. A dense tantalum carbide coating can be formed by powder sintering, but powder sintering has the problem of cracks caused by the stress of sintering shrinkage of the dense powder film and the constraints from the substrate.

[0003] At present, the TaC coating (tantalum carbide coating) on ​​the surface of the crucible can be formed by coating tantalum carbide powder slurry and then sintering to reduce the risk of cracks in the tantalum carbide coating. However, this method has the problem of low carbon content in the sintered tantalum carbide coating; in addition, the density of tantalum carbide powder is large, and it is easy to settle, which reduces the stability of the slurry and causes defects in the coating after sintering due to uneven density; and the powder in the tantalum carbide slurry is fine and easy to agglomerate, and it is not easy to disperse, resulting in a low solid content, which reduces the density of the sintered coating. Summary of the invention

[0004] Based on this, it is necessary to provide a tantalum carbide slurry with good stability and the ability to form a higher stacking density and a preparation method thereof, as well as a tantalum carbide coating with higher density and fewer cracks prepared using the tantalum carbide slurry and a preparation method thereof and a crucible.

[0005] A first aspect of the present invention provides a tantalum carbide slurry, which comprises, by weight, 70 to 80 parts of modified tantalum carbide, 0.5 to 1.0 parts of a sintering aid, 0.5 to 1.0 parts of a binder, and 18.5 to 28 parts of a solvent; the modified tantalum carbide comprises tantalum carbide and a polymer resin layer, and the polymer resin layer is coated on the surface of the tantalum carbide.

[0006] The above-mentioned tantalum carbide slurry, by matching the components according to a specific ratio, forms a slurry with good stability, high tantalum carbide content, and the ability to form a coating layer with a high stacking density; the slurry can form a tantalum carbide coating with a high carbon content, high density, and few cracks. Specifically, the use of a polymer resin layer to coat tantalum carbide can prevent the agglomeration of tantalum carbide, so that the modified tantalum carbide powder has better dispersibility in the tantalum carbide slurry; it can also prevent the sedimentation of tantalum carbide to a certain extent, improve the stability of the tantalum carbide slurry, thereby forming a uniform and stable coating layer, and further improve the uniformity of the tantalum carbide coating structure; at the same time, the polymer resin layer will be in-situ cracked into activated carbon on the surface of the tantalum carbide powder during the subsequent sintering process, which can react with the oxygen on the surface of the tantalum carbide powder to form a carbonization reaction, thereby making the tantalum carbide coating have a higher carbon content. Further controlling the content of modified tantalum carbide in the slurry can significantly reduce the shrinkage rate and thermal stress of the sintered tantalum carbide coating, avoid the generation of cracks, and further improve the density of the tantalum carbide coating.

[0007] In some embodiments, the tantalum carbide slurry satisfies at least one of the following conditions:

[0008] (1) The average particle size of the tantalum carbide is 0.2 μm to 3.0 μm;

[0009] (2) The thickness of the polymer resin layer is 5 nm to 10 nm;

[0010] (3) The mass of the polymer resin layer is 1wt% to 3wt% of the mass of the tantalum carbide.

[0011] In some embodiments, the tantalum carbide slurry satisfies at least one of the following conditions:

[0012] (1) The material of the polymer resin layer is epoxy resin;

[0013] (2) The binder is selected from non-ionic polymer binders;

[0014] (3) The average particle size of the sintering aid is 50nm~800nm;

[0015] (4) The sintering aid is selected from at least one of tantalum disilicide, molybdenum disilicide, pyrolytic carbon black, aluminum oxide and yttrium oxide.

[0016] In some embodiments, the tantalum carbide is surface hydroxylated tantalum carbide; and / or,

[0017] The modified tantalum carbide further includes a non-ionic surfactant, and the non-ionic surfactant is connected to the surface of the polymer resin layer.

[0018] In some embodiments, the nonionic surfactant is selected from at least one of dipropylene triamine and coconut fatty acid diethylamide.

[0019] In some embodiments, the component further comprises 0.5 parts to 2.0 parts of a plasticizer.

[0020] A second aspect of the present invention provides a method for preparing the above-mentioned tantalum carbide slurry, comprising the following steps:

[0021] The components are mixed to obtain tantalum carbide slurry.

[0022] In some embodiments, the preparation method further includes a preparation step of modified tantalum carbide, including:

[0023] The tantalum carbide is subjected to hydroxylation treatment to obtain tantalum carbide with surface hydroxylation;

[0024] The surface of the hydroxylated tantalum carbide is coated with a polymer resin to obtain tantalum carbide with a polymer resin layer coated on the surface.

[0025] In some embodiments, the preparation step of the modified tantalum carbide further comprises:

[0026] The step of connecting a nonionic surfactant to the surface of tantalum carbide coated with a polymer resin layer.

[0027] A third aspect of the present invention provides a tantalum carbide coating, wherein the raw materials for preparing the tantalum carbide coating include the above-mentioned tantalum carbide slurry.

[0028] A fourth aspect of the present invention provides a method for preparing a tantalum carbide coating, comprising the following steps:

[0029] The tantalum carbide slurry is coated on the surface of the substrate and then sintered.

[0030] In some embodiments, the sintering treatment temperature is 2100° C. to 2300° C., and the holding time is 10 min to 120 min.

[0031] A fifth aspect of the present invention provides a crucible, comprising a crucible body and the tantalum carbide coating provided on the surface of the crucible body. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the microstructural morphology of the tantalum carbide coating prepared in Example 1.

[0033] Figure 2 This is a macroscopic photograph of a crucible with a tantalum carbide coating prepared in Example 1. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present invention, the present invention is described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0036] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0037] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0038] In one embodiment of the present invention, a tantalum carbide slurry is provided, wherein the components thereof include 70 to 80 parts of modified tantalum carbide, 0.5 to 1.0 parts of a sintering aid, 0.5 to 1.0 parts of a binder, and 18.5 to 28 parts of a solvent, by weight; the modified tantalum carbide includes tantalum carbide and a polymer resin layer, and the polymer resin layer is coated on the surface of the tantalum carbide.

[0039] The above-mentioned tantalum carbide slurry, by matching the components according to a specific ratio, forms a slurry with good stability, high tantalum carbide content, and the ability to form a coating layer with a high stacking density; the slurry can form a tantalum carbide coating with a high carbon content, high density, and few cracks. Specifically, the use of a polymer resin layer to coat tantalum carbide can prevent the agglomeration of tantalum carbide, so that the modified tantalum carbide powder has better dispersibility in the tantalum carbide slurry; it can also prevent the sedimentation of tantalum carbide to a certain extent, improve the stability of the tantalum carbide slurry, thereby forming a uniform and stable coating layer, and further improve the uniformity of the tantalum carbide coating structure; at the same time, the polymer resin layer will be in-situ cracked into activated carbon on the surface of the tantalum carbide powder during the subsequent sintering process, which can react with the oxygen on the surface of the tantalum carbide powder to form a carbonization reaction, thereby making the tantalum carbide coating have a higher carbon content. Further controlling the content of modified tantalum carbide in the slurry can significantly reduce the shrinkage rate and thermal stress of the sintered tantalum carbide coating, avoid the generation of cracks, and further improve the density of the tantalum carbide coating.

[0040] The above “70 to 80 parts of modified tantalum carbide” can be understood as the number of modified tantalum carbide can be 70, 72, 74, 75, 76, 78 or 80 parts. Further, the number of modified tantalum carbide can be a range value formed between any two of the above point values. Preferably, the number of modified tantalum carbide is 72 to 78 parts.

[0041] The above “0.5 to 1.0 parts of sintering aid” can be understood as the amount of sintering aid can be 0.5, 0.6, 0.7, 0.8, 0.9 or 1. Further, the amount of sintering aid can be a range value formed between any two of the above point values.

[0042] The above “0.5 to 1.0 parts of binder” can be understood as the number of parts of the binder can be 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts or 1 parts. Further, the number of parts of the binder can be a range value formed between any two of the above point values.

[0043] The above “18.5 to 28 parts of solvent” can be understood as the number of parts of the solvent can be 18.5, 19.8, 20, 25 or 28. Further, the number of parts of the solvent can be a range value formed between any two of the above point values. Preferably, the number of parts of the solvent is 19 to 26 parts.

[0044] In some embodiments, the average particle size of tantalum carbide is 0.2 μm to 3.0 μm. It is understood that the average particle size of tantalum carbide is 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm or 3.0 μm. Further, the average particle size of tantalum carbide can be a range value consisting of any two of the above point values. Preferably, the average particle size of tantalum carbide is 0.8 μm to 2.5 μm. By controlling the average particle size of tantalum carbide, the viscosity of the slurry can be effectively regulated to achieve uniform spraying or coating treatment.

[0045] In some embodiments, the thickness of the polymer resin layer in the modified tantalum carbide is 5 nm to 10 nm. It is understood that the thickness of the polymer resin layer in the modified tantalum carbide can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm. Further, the thickness of the polymer resin layer in the modified tantalum carbide can be a range value consisting of any two of the above point values. Preferably, the thickness of the polymer resin layer in the modified tantalum carbide is 6 nm to 8 nm.

[0046] In some embodiments, the mass of the polymer resin layer is 1wt% to 3wt% of the mass of the tantalum carbide. By controlling the mass of the polymer resin layer on the surface of the tantalum carbide, the dispersion of the tantalum carbide particles can be further controlled, thereby improving the stability of the tantalum carbide slurry. At the same time, the carbon content of the tantalum carbide coating can also be further increased.

[0047] In some embodiments, the average particle size of the sintering aid is 50nm~800nm. It is understood that the average particle size of the sintering aid is 50nm, 100nm, 200nm, 300nm, 400nm, 500nm, 700nm or 800nm. Further, the average particle size of the sintering aid can be a range value consisting of any two of the above point values. Preferably, the average particle size of the sintering aid is 50nm~200nm.

[0048] In some embodiments, the sintering aid is selected from at least one of tantalum disilicide, molybdenum disilicide, pyrolytic carbon black, aluminum oxide, and yttrium oxide. Preferably, the sintering aid is selected from at least one of tantalum disilicide and molybdenum disilicide.

[0049] In some embodiments, the material of the polymer resin layer is epoxy resin.

[0050] In some embodiments, the epoxy resin is selected from at least one of bisphenol A epoxy resin, diglycidyl ether, hydantoin epoxy resin, phenolic resin and polyester resin. Preferably, the epoxy resin is hydantoin epoxy resin.

[0051] In some embodiments, the binder is selected from non-ionic polymer binders.

[0052] In some embodiments, the binder is selected from at least one of polyacrylamide, polyethylene oxide, polyurethane, polyvinyl alcohol, polyaniline, and polyethylene terephthalate.

[0053] In some embodiments, the solvent is selected from at least one of ether, anhydrous ethanol, butanone, n-octanol, triolein, toluene, xylene, and isopropanol.

[0054] In some embodiments, the tantalum carbide is surface hydroxylated tantalum carbide.

[0055] In some embodiments, the modified tantalum carbide further comprises a nonionic surfactant, and the nonionic surfactant is connected to the surface of the polymer resin layer. Connecting the nonionic surfactant to the surface of the polymer resin layer can further improve the dispersibility between the modified tantalum carbides, thereby improving the stability of the tantalum carbide slurry.

[0056] In some embodiments, in some embodiments, the nonionic surfactant is selected from at least one of dipropylene triamine (TCI) and coconut fatty acid diethylamide. Preferably, the nonionic surfactant is dipropylene triamine (TCI).

[0057] In some embodiments, the components of the tantalum carbide slurry further include 0.5 parts to 2.0 parts of a plasticizer.

[0058] The above “0.5 to 2.0 parts of plasticizer” can be understood as the plasticizer can be 0.5 parts, 1.0 parts or 2.0 parts. Further, the number of parts of the plasticizer can be a range value formed between any two of the above point values.

[0059] In some embodiments, the total weight of the modified tantalum carbide, sintering aid, binder, solvent and plasticizer in the tantalum carbide slurry is 100 parts. It is understood that in some examples, the plasticizer may also be omitted.

[0060] In some embodiments, the components of the tantalum carbide slurry include, by weight percentage, 70 wt% to 80 wt% of modified tantalum carbide, 0.5 wt% to 1.0 wt% of sintering aid, 0.5 wt% to 1.0 wt% of binder, 18.5 wt% to 28 wt% of solvent, and 0.5 wt% to 2.0 wt% of plasticizer. Preferably, by weight percentage, the components of the tantalum carbide slurry include 72 wt% to 78 wt% of modified tantalum carbide, 0.5 wt% to 1.0 wt% of sintering aid, 0.5 wt% to 1.0 wt% of binder, 19 wt% to 26 wt% of solvent, and 0.5 wt% to 2.0 wt% of plasticizer.

[0061] In some embodiments, the plasticizer is selected from at least one of polyethylene glycol, dibutyl phthalate, methylcellulose, phthalate esters, and epoxidized soybean oil.

[0062] In one embodiment, a method for preparing the above-mentioned tantalum carbide slurry is provided, comprising the following preparation steps:

[0063] The components of the above tantalum carbide slurry are mixed to obtain tantalum carbide slurry.

[0064] In some embodiments, the method for preparing tantalum carbide slurry further comprises the step of ball milling the mixture after mixing the components of the tantalum carbide slurry. Ball milling the mixture is beneficial to homogenizing the powder particles in the slurry, further preventing the local viscosity of the slurry caused by soft agglomeration and reducing the stability of the slurry.

[0065] In some embodiments, the ball milling is performed by wet ball milling.

[0066] In some embodiments, the dispersion medium for ball milling is anhydrous ethanol or deionized water.

[0067] In some embodiments, the ball milling medium is selected from at least one of silicon carbide balls, zirconium oxide balls, agate balls, quartz balls, stainless steel balls, and corundum balls.

[0068] In some embodiments, the ball-to-material ratio of ball milling is (1-5):1. The ball-to-material ratio refers to the ratio of the mass of the ball milling medium to the total mass of the component raw materials. Further, the ball-to-material ratio is (2-3):1.

[0069] In some embodiments, the ball milling time is 2 h to 6 h.

[0070] In some embodiments, the ball milling speed is 50 r / min to 500 r / min. Further, the ball milling speed is 80 r / min to 160 r / min.

[0071] In some embodiments, the method for preparing tantalum carbide slurry further includes a step of preparing modified tantalum carbide, which includes the following steps S10-S20:

[0072] S10, subjecting the tantalum carbide to a hydroxylation treatment to obtain tantalum carbide with a hydroxylated surface;

[0073] S20, coating the surface of the tantalum carbide with hydroxylation with a polymer resin to obtain tantalum carbide with a polymer resin layer coated on the surface.

[0074] In some embodiments, the hydroxylation treatment of tantalum carbide in the above step S10 includes the following steps S11-S12.

[0075] S11, pouring tantalum carbide into a hydrogen peroxide solution, performing dispersion treatment, and obtaining a first mixed material.

[0076] S12, reflux the first mixed material at 100° C. to 120° C. for 4 h to 12 h; then perform solid-liquid separation, collect solid particles and wash them to obtain tantalum carbide with surface hydroxylation.

[0077] In some embodiments, the concentration of hydrogen peroxide in the hydrogen peroxide solution is 10 wt % to 30 wt %.

[0078] In some embodiments, the dispersion process may be performed by stirring or ultrasonic treatment.

[0079] In some embodiments, the dispersion treatment time is 30 min to 60 min.

[0080] In some embodiments, the solid-liquid separation may be performed by centrifugal sedimentation.

[0081] In some embodiments, the centrifugal sedimentation time is 5 min to 30 min.

[0082] In some embodiments, the method of coating the surface of the hydroxylated tantalum carbide with a polymer resin in the above step S20 includes the following steps S21-S22.

[0083] S21, pouring the surface hydroxylated tantalum carbide into the polymer resin solution to obtain a suspension;

[0084] S22. Add a pH adjuster to the suspension to adjust the pH value of the suspension to 1-3, and perform a first reaction.

[0085] In some embodiments, the concentration of the polymer resin in the polymer resin solution is 2 wt % to 8 wt %.

[0086] In some embodiments, the pH adjuster is selected from at least one of dilute hydrochloric acid and dilute sulfuric acid.

[0087] In some embodiments, the temperature of the first reaction is 40°C to 80°C.

[0088] In some embodiments, the first reaction time is 2 h to 4 h.

[0089] In some embodiments, the step of preparing modified tantalum carbide further includes the following step S30.

[0090] S30, connecting a nonionic surfactant to the surface of the tantalum carbide coated with the polymer resin layer.

[0091] In some embodiments, the method of connecting a non-ionic surfactant to the surface of tantalum carbide coated with a polymer resin layer comprises the following step S31:

[0092] S31. After the first reaction in the above step S22 is completed, add a nonionic surfactant, stir at room temperature for 8h~24h, and then stir at 60℃~100℃ for 1h~4h.

[0093] In some embodiments, after the step of connecting a non-ionic surfactant to the surface of tantalum carbide coated with a polymer resin layer, the steps of solid-liquid separation, washing and drying are also included.

[0094] In some embodiments, the above-mentioned cleaning may use deionized water to clean the solid particles.

[0095] In some embodiments, the drying condition may be vacuum drying at 40° C. to 80° C.

[0096] In some embodiments, the drying time is 8 hours to 24 hours.

[0097] In one embodiment of the present invention, a tantalum carbide coating is provided, and the raw materials for preparing the tantalum carbide coating include the above-mentioned tantalum carbide slurry.

[0098] In one embodiment of the present invention, a method for preparing a tantalum carbide coating is provided, comprising the following preparation steps:

[0099] The tantalum carbide slurry is coated on the surface of the substrate and then sintered.

[0100] In some embodiments, the coating method may be spray coating, brush coating or dipping coating.

[0101] In some embodiments, the tantalum carbide slurry is coated on the surface of the substrate to form a coating layer, and the thickness of the coating layer is 35 μm to 60 μm.

[0102] In some embodiments, after coating the tantalum carbide slurry on the surface of the substrate and before sintering, a step of drying the coating layer is also included.

[0103] In some embodiments, the drying condition may be vacuum drying at 40° C. to 80° C.

[0104] In some embodiments, the drying time is 8 hours to 24 hours.

[0105] In some embodiments, the bulk density of the coating layer after drying is 65 vol% to 70 vol%.

[0106] In some embodiments, the sintering temperature is 2100° C. to 2300° C., and the holding time is 10 min to 120 min.

[0107] In some embodiments, the sintering process is performed under protective gas conditions.

[0108] In some embodiments, the protective gas is at least one of hydrogen and nitrogen.

[0109] In one embodiment of the present invention, a crucible is provided. The crucible includes a crucible body and the tantalum carbide coating disposed on the surface of the crucible body.

[0110] In some embodiments, the tantalum carbide coating in the crucible is disposed on the inner surface and the outer surface of the crucible body. The outer surface includes the outer wall and the bottom of the crucible body.

[0111] In some embodiments, the thickness of the tantalum carbide coating in the crucible is 30 μm to 50 μm.

[0112] In some embodiments, the density of the tantalum carbide coating in the crucible is greater than or equal to 97.5%.

[0113] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0114] In order to better illustrate the present invention, the present invention is further described below in conjunction with the embodiments. The following are specific embodiments. Example 1

[0115] Surface modification of tantalum carbide:

[0116] (1) Tantalum carbide particles with a particle size of 0.8 μm were poured into a 10 wt% H2O2 aqueous solution and ultrasonically dispersed for 30 min, then heated to 105°C and refluxed for 6 h. The tantalum carbide particles were then collected by centrifugal sedimentation for 10 min and washed with deionized water to obtain surface hydroxylated tantalum carbide particles.

[0117] (2) The surface hydroxylated tantalum carbide particles obtained in step (1) are poured into a 3 wt % aqueous solution of hydantoin epoxy resin (product model: MHR-070) so that the mass of hydantoin epoxy resin is 1 wt % of the total mass of the tantalum carbide particles. Dilute sulfuric acid is then added to make the pH value of the mixture 1.0. The mixture is then stirred at 60° C. for 2 h to obtain a suspension of tantalum carbide particles having a surface coated with an epoxy resin layer.

[0118] (3) Add 1wt% of dipropylene triamine (TCI) to the suspension in step (4), and stir at room temperature for 16h, and then stir at 60°C for 2h. Then centrifuge and collect silicon carbide nanoparticles, wash tantalum carbide with deionized water, and vacuum dry at 60°C for 12h to obtain modified tantalum carbide. The thickness of the surface resin layer of the modified tantalum carbide is 5~10nm.

[0119] Preparation method of tantalum carbide slurry:

[0120] (1) Raw materials are weighed and set aside according to the formula, the specific formula being: 72.0 parts of modified tantalum carbide powder, 0.5 parts of tantalum disilicide powder, 0.5 parts of polyvinyl alcohol, 26.0 parts of triolein and 1.0 parts of phthalate. The average particle size of the tantalum disilicide powder is 100 nm.

[0121] (2) The raw materials weighed in step (1) are mixed and wet-milled, wherein the ball milling time is 2 h, the ball-to-material ratio is 2:1, and the rotation speed is 120 r / min to obtain tantalum carbide slurry.

[0122] Preparation method of tantalum carbide coating:

[0123] (1) The tantalum carbide slurry prepared in the above steps is evenly coated on the inner and outer surfaces of the crucible by spraying, and the thickness of the coating layer is 60 μm.

[0124] (2) Place the sprayed crucible in a vacuum drying oven for drying at a temperature of 50°C for 8 hours.

[0125] (3) Place the dried crucible in a sintering furnace, introduce a mixture of high-purity hydrogen and high-purity argon, wherein the hydrogen content is 3% and the argon content is 97%; heat it to 2150°C at a rate of 3°C / min and keep it for 60 minutes for high-temperature sintering. Then cool it to room temperature with the furnace to obtain a crucible product with a high-density and high-uniform tantalum carbide sintered coating. Example 2

[0126] Surface modification of tantalum carbide:

[0127] (1) Tantalum carbide particles with an average particle size of 0.8 μm were poured into a 20 wt% H2O2 aqueous solution and ultrasonically dispersed for 40 min, then heated to 110°C and refluxed for 6 h. The tantalum carbide particles were then collected by centrifugal sedimentation for 20 min and washed with deionized water to obtain surface hydroxylated tantalum carbide particles.

[0128] (2) The surface hydroxylated tantalum carbide particles obtained in step (1) are poured into a 6 wt % aqueous solution of hydantoin epoxy resin (product model: MHR-070) so that the mass of hydantoin epoxy resin is 2 wt % of the total mass of the tantalum carbide particles, and then dilute sulfuric acid is added to make the pH value of the mixed solution 1.5, and then stirred at 60° C. for 2 h to obtain a suspension of tantalum carbide particles with a surface coated with an epoxy resin layer.

[0129] (3) Add 2 wt% of dipropylene triamine (TCI) to the suspension in step (4), and stir at room temperature for 20 h, and then stir at 60°C for 2 h. Then centrifuge and collect the tantalum carbide particles, wash the tantalum carbide particles with deionized water, and vacuum dry at 60°C for 8 h to obtain modified tantalum carbide. The thickness of the surface resin layer of the modified tantalum carbide is 6 nm to 8 nm.

[0130] Preparation method of tantalum carbide slurry:

[0131] (1) Raw materials were weighed and set aside according to the formula, and the specific formula was: 76.0 parts of modified tantalum carbide powder, 0.3 parts of tantalum disilicide powder, 0.3 parts of molybdenum disilicide powder, 0.6 parts of polyacrylamide, 22.2 parts of xylene and 0.6 parts of epoxidized soybean oil. The average particle size of the tantalum disilicide powder was 80 nm, and the average particle size of the molybdenum disilicide powder was 200 nm.

[0132] (2) The raw materials weighed in step (1) are mixed and wet-milled, wherein the ball milling time is 4 h, the ball-to-material ratio is 2:1, and the rotation speed is 120 r / min to obtain tantalum carbide slurry.

[0133] Preparation method of tantalum carbide coating:

[0134] (1) The tantalum carbide slurry prepared in the above steps is evenly coated on the inner and outer surfaces of the crucible by spraying, and the thickness of the coating layer is 50 μm.

[0135] (2) Place the sprayed crucible in a vacuum drying oven for drying at a temperature of 60°C for 8 hours.

[0136] (3) Place the dried crucible in a sintering furnace, introduce a mixture of high-purity hydrogen and high-purity argon, wherein the hydrogen content is 4% and the argon content is 96%; heat it to 2200°C at a rate of 5°C / min and keep it at that temperature for 30 minutes for high-temperature sintering. Then cool it to room temperature with the furnace to obtain a crucible product with a high-density and high-uniform tantalum carbide sintered coating. Example 3

[0137] Surface modification of tantalum carbide:

[0138] (1) Tantalum carbide particles with an average particle size of 1.5 μm were poured into a 30 wt% H2O2 aqueous solution and ultrasonically dispersed for 60 min, then heated to 120°C and refluxed for 8 h. The tantalum carbide particles were then collected by centrifugal sedimentation for 30 min and washed with deionized water to obtain surface hydroxylated tantalum carbide particles.

[0139] (2) The surface hydroxylated tantalum carbide particles obtained in step (1) are poured into an 8 wt % aqueous solution of hydantoin epoxy resin (product model: MHR-070) so that the mass of hydantoin epoxy resin is 3 wt % of the total mass of the tantalum carbide particles. Dilute sulfuric acid is then added to make the pH value of the mixed solution 1.5. The mixture is then stirred at 60° C. for 2 h to obtain a suspension of tantalum carbide particles having a surface coated with an epoxy resin layer.

[0140] (3) Add 3 wt% of dipropylene triamine (TCI) to the suspension in step (4), and stir at room temperature for 20 h, and then stir at 60°C for 4 h. Then centrifuge and collect the tantalum carbide particles, wash the tantalum carbide particles with deionized water, and vacuum dry at 60°C for 12 h to obtain modified tantalum carbide. The thickness of the surface resin layer of the modified tantalum carbide is 5 nm to 8 nm.

[0141] Preparation method of tantalum carbide slurry:

[0142] (1) Weigh the raw materials according to the formula, and set aside. The specific formula is: 78.0 parts of modified tantalum carbide powder, 0.5 parts of tantalum disilicide powder, 0.3 parts of pyrolytic carbon black powder, 0.8 parts of polyacrylamide, 19.8 parts of n-octanol and 0.6 parts of polyethylene glycol. Among them, the average particle size of tantalum disilicide powder is 150nm, the average particle size of molybdenum disilicide powder is 80nm, and the average particle size of pyrolytic carbon black powder is 50nm.

[0143] (2) The raw materials weighed in step (1) are mixed and wet-milled, wherein the ball milling time is 5 h, the ball-to-material ratio is 3:1, and the rotation speed is 160 r / min to obtain tantalum carbide slurry.

[0144] Preparation method of tantalum carbide coating:

[0145] (1) The tantalum carbide slurry prepared in the above steps is evenly coated on the inner and outer surfaces of the crucible by spraying, and the thickness of the coating layer is 35 μm.

[0146] (2) Place the sprayed crucible in a vacuum drying oven for drying at a temperature of 60°C for 8 hours.

[0147] (3) Place the dried crucible in a sintering furnace, introduce a mixture of high-purity hydrogen and high-purity argon, wherein the hydrogen content is 5% and the argon content is 95%; heat to 2250°C at a rate of 3°C / min and keep at that temperature for 20 minutes for high-temperature sintering. Then cool to room temperature with the furnace to obtain a crucible product with a high-density and high-uniform tantalum carbide sintered coating. Example 4

[0148] The preparation method of this embodiment is consistent with that of embodiment 1, except that the formula of the tantalum carbide slurry in this embodiment is different. Specifically, the formula of the tantalum carbide slurry is 70 parts of modified tantalum carbide powder, 1.0 part of tantalum disilicide powder, 1.0 part of polyvinyl alcohol, 27 parts of triolein and 1.0 part of phthalate, wherein the average particle size of the tantalum disilicide powder is 100 nm. Other process conditions and parameters are consistent with those of embodiment 1. Example 5

[0149] The preparation method of this embodiment is consistent with that of embodiment 1, except that step (3) is omitted in the preparation of the modified tantalum carbide in this embodiment, that is, the surface of the modified tantalum carbide in this embodiment is not connected with a non-ionic surfactant. Other process conditions and parameters are consistent with those of embodiment 1. Example 6

[0150] The preparation method of this embodiment is consistent with that of embodiment 1, and the only difference is that the polymer resin solution used in step (2) of this embodiment is different when preparing the modified tantalum carbide. Specifically, step (2) of this embodiment is: pouring the surface hydroxylated tantalum carbide particles obtained in step (1) into a 3wt% aqueous solution of bisphenol A epoxy resin (product model: EP01441-310) so that the mass of bisphenol A epoxy resin is 1wt% of the total mass of the tantalum carbide particles, then adding dilute sulfuric acid so that the pH value of the mixed solution is 1.0, and then stirring at 60°C for 2h to obtain a suspension of tantalum carbide particles with a surface coated with an epoxy resin layer. Other process conditions and parameters are consistent with those of embodiment 1.

[0151] Comparative Example 1

[0152] The preparation method of this comparative example is basically the same as that of Example 1, except that the step of surface modification of tantalum carbide is omitted in this comparative example, and the modified tantalum carbide powder in Example 1 is directly replaced with unmodified tantalum carbide of equal mass in the preparation step of tantalum carbide slurry in this comparative example. Other process conditions and parameters are the same as those in Example 1.

[0153] Comparative Example 2

[0154] The preparation method of this comparative example is basically the same as that of Example 1, except that the formula of the tantalum carbide slurry is different, and no sintering aid is added in this comparative example. Specifically, the formula of the tantalum carbide slurry in this comparative example is: 72.5 parts of modified tantalum carbide powder, 0.5 parts of polyvinyl alcohol, 26.0 parts of triolein, and 1.0 parts of phthalate. Other process conditions and parameters are the same as those in Example 1.

[0155] Comparative Example 3

[0156] Surface modification of tantalum carbide:

[0157] (1) Tantalum carbide particles with an average particle size of 1.2 μm were poured into a 20 wt% H2O2 aqueous solution and ultrasonically dispersed for 40 min, then heated to 110°C and refluxed for 6 h. The tantalum carbide particles were then collected by centrifugal sedimentation for 40 min and washed with deionized water to obtain surface hydroxylated tantalum carbide particles.

[0158] (2) The surface hydroxylated tantalum carbide particles obtained in step (1) are poured into a 6 wt % aqueous solution of hydantoin epoxy resin (product model: MHR-070) so that the mass of hydantoin epoxy resin is 2 wt % of the total mass of the tantalum carbide particles, and then dilute sulfuric acid is added to make the pH value of the mixed solution 1.5, and then stirred at 60° C. for 2 h to obtain a suspension of tantalum carbide particles with a surface coated with an epoxy resin layer.

[0159] (3) Add 2 wt% of dipropylene triamine (TCI) to the suspension in step (4), and stir at room temperature for 20 h, and then stir at 60° C. for 2 h. Then centrifuge and collect the tantalum carbide particles, wash the tantalum carbide particles with deionized water, and vacuum dry them at 60° C. for 8 h to obtain modified tantalum carbide.

[0160] Preparation method of tantalum carbide slurry:

[0161] (1) Weigh the raw materials according to the formula, and set aside. The specific formula is: 66.0 parts of modified tantalum carbide powder, 0.3 parts of tantalum disilicide powder, 0.3 parts of molybdenum disilicide powder, 0.6 parts of polyacrylamide, 32.2 parts of xylene and 0.6 parts of epoxidized soybean oil. Among them, the average particle size of tantalum disilicide powder is 150nm, the average particle size of molybdenum disilicide powder is 80nm, and the average particle size of pyrolytic carbon black powder is 50nm.

[0162] (2) The raw materials weighed in step (1) are mixed and wet-milled, wherein the ball milling time is 4 h, the ball-to-material ratio is 2:1, and the rotation speed is 120 r / min to obtain tantalum carbide slurry.

[0163] Preparation method of tantalum carbide coating:

[0164] (1) The tantalum carbide slurry prepared in the above steps is evenly coated on the inner and outer surfaces of the crucible by spraying, and the thickness of the coating layer is 35 μm.

[0165] (2) Place the sprayed crucible in a vacuum drying oven for drying at a temperature of 60°C for 8 hours.

[0166] (3) Place the dried crucible in a sintering furnace, introduce a mixture of high-purity hydrogen and high-purity argon, wherein the hydrogen content is 4% and the argon content is 96%; heat it to 2200°C at a rate of 3°C / min and keep it at that temperature for 30 minutes for high-temperature sintering. Then cool it to room temperature with the furnace to obtain a crucible product with a high-density and high-uniform tantalum carbide sintered coating.

[0167] Comparative Example 4

[0168] The preparation method of this comparative example is basically the same as that of Example 3, except that no binder is added when preparing the tantalum carbide slurry prepared in this comparative example. Specifically, the formula of the tantalum carbide slurry in this comparative example is: 78.8 parts of modified tantalum carbide powder, 0.5 parts of tantalum disilicide powder, 0.3 parts of pyrolytic carbon black powder, 19.8 parts of n-octanol and 0.6 parts of polyethylene glycol. Among them, the average particle size of tantalum disilicide powder is 150nm, the average particle size of molybdenum disilicide powder is 80nm, and the average particle size of pyrolytic carbon black powder is 50nm.

[0169] Performance Testing Methods

[0170] Slurry suspension stability time: tested according to the method specified in GB / T 26645.4-2018.

[0171] Density of sintered tantalum carbide coating: The density of sintered tantalum carbide coating is tested according to the method specified in GB / T 39688-2020.

[0172] Average thickness of coating after sintering: Test the thickness of the coating at 5 different locations according to the method specified by the microstructure line section method, and take the average value. The test steps of the microstructure line section method are as follows: 1) Use a ruler with a length of 20μm on the scanning electron microscope photo (500×), 2) Use a line segment tool to draw a line segment perpendicular to the coating surface that intersects the edge of the coating thickness; 3) Compare the line segment with the 20μm ruler to determine the thickness of the cut coating.

[0173] The performance test data of each embodiment and comparative example are shown in Table 1:

[0174] Table 1

[0175]

[0176] As can be seen from Table 1, the tantalum carbide slurry suspension prepared in Examples 1-6 has good stability of 40h~60h, the average thickness of the coating after sintering is high, the density of the tantalum carbide coating also reaches 96.5%~98.5%, and no cracks are generated. Figure 1 The microstructure of the tantalum carbide coating prepared in Example 1 is shown in FIG. Figure 2 The crucible containing tantalum carbide coating prepared in Example 1 shown has a uniform coating on the surface and a fine color.

[0177] Compared with Example 1, the difference between Comparative Example 1 is that Comparative Example 1 does not perform surface modification on the tantalum carbide particles, but directly mixes the unmodified tantalum carbide with a sintering aid, a binder and a solvent to form a tantalum carbide slurry. The suspension stability time of the obtained tantalum carbide slurry is only 12 hours; the thickness of the sintered tantalum carbide coating is reduced by 10 μm compared with the thickness of the coating layer, the density of the obtained tantalum carbide coating is also lower than that of Example 1, and cracks appear in the tantalum carbide coating.

[0178] The difference between Comparative Example 2 and Example 1 is that no sintering aid is added in Comparative Example 2, the suspension stability of the obtained slurry is not as good as that in Example 1, fine cracks are generated in the prepared tantalum carbide coating, and the density of the tantalum carbide coating is also not as good as that in Example 1.

[0179] When preparing tantalum carbide slurry in Comparative Example 3, the content of the component added to the modified tantalum carbide is low, the obtained tantalum carbide coating has low density, and cracks are generated. Compared with Example 3, Comparative Example 4 is different in that no binder component is added when preparing tantalum carbide slurry in Comparative Example 4, the suspension stability time of the obtained tantalum carbide slurry is only 8 hours, and the prepared tantalum carbide coating also has cracks.

[0180] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0181] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A tantalum carbide slurry, characterized in that: The components include 70 to 80 parts of modified tantalum carbide, 0.5 to 1.0 parts of sintering aid, 0.5 to 1.0 parts of binder and 18.5 to 28 parts of solvent by weight; The modified tantalum carbide comprises tantalum carbide, a polymer resin layer and a nonionic surfactant; the tantalum carbide is tantalum carbide with surface hydroxylation; the polymer resin layer is coated on the surface of the tantalum carbide; the nonionic surfactant is connected to the surface of the polymer resin layer; The material of the polymer resin layer is selected from at least one of bisphenol A epoxy resin and hydantoin epoxy resin; the mass of the polymer resin layer is 1wt% to 3wt% of the mass of the tantalum carbide; The nonionic surfactant is selected from at least one of dipropylene triamine and coconut fatty acid diethylamide.

2. The tantalum carbide slurry according to claim 1, characterized in that The tantalum carbide slurry satisfies at least one of the following conditions: (1) The average particle size of the tantalum carbide is 0.2 μm to 3.0 μm; (2) The thickness of the polymer resin layer is 5 nm to 10 nm.

3. The tantalum carbide slurry according to any one of claims 1 to 2, characterized in that The tantalum carbide slurry satisfies at least one of the following conditions: (1) The binder is selected from non-ionic polymer binders; (2) The average particle size of the sintering aid is 50nm~800nm; (3) The sintering aid is selected from at least one of tantalum disilicide, molybdenum disilicide, pyrolytic carbon black, aluminum oxide and yttrium oxide.

4. The tantalum carbide slurry according to any one of claims 1 to 2, characterized in that: The components also include 0.5 to 2.0 parts of a plasticizer.

5. The method for preparing tantalum carbide slurry according to any one of claims 1 to 4, characterized in that: The steps include: The components are mixed to obtain tantalum carbide slurry.

6. The method for preparing tantalum carbide slurry according to claim 5, characterized in that: The preparation method also includes a preparation step of modified tantalum carbide, including: The tantalum carbide is subjected to hydroxylation treatment to obtain tantalum carbide with surface hydroxylation; The surface of the hydroxylated tantalum carbide is coated with a polymer resin to obtain tantalum carbide with a polymer resin layer coated on the surface.

7. The preparation method according to any one of claims 5 to 6, characterized in that The preparation steps of the modified tantalum carbide also include: The step of connecting a nonionic surfactant to the surface of tantalum carbide coated with a polymer resin layer.

8. A tantalum carbide coating, characterized in that: The raw material for preparing the tantalum carbide coating includes the tantalum carbide slurry as described in any one of claims 1 to 4.

9. The method for preparing a tantalum carbide coating according to claim 8, characterized in that: The steps include: The tantalum carbide slurry is coated on the surface of the substrate and then sintered.

10. The preparation method according to claim 9, characterized in that: The sintering treatment temperature is 2100° C. to 2300° C., and the heat preservation time is 10 min to 120 min.

11. A crucible, characterized in that: The crucible comprises a crucible body and the tantalum carbide coating as claimed in claim 8 disposed on the surface of the crucible body.