A method for preparing amorphous multi-level porous UiO-66

Amorphous hierarchical porous UiO-66 was prepared through coordination reaction under cell survival conditions at 15-37°C and normal pressure, which solved the problem of harsh preparation conditions in the existing technology and achieved biocompatibility, simplicity and efficiency. The process provides new material applications for the biomedical field.

CN118063785BActive Publication Date: 2024-10-08SHENZHEN POLYTECHNIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410295395.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-10-08
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

It is difficult to prepare amorphous UiO-66 under cell survival conditions with existing technology, resulting in its inability to be used in the biological field.

Method used

The amorphous state is achieved by mixing polyethylene glycol, zirconium nitrate and water at 15 to 37°C and normal pressure to form a metal solution, and then mixing it with ammonium fluoride, terephthalic acid and water to perform a coordination reaction. Preparation of hierarchical porous UiO-66. This method simplifies the process and avoids harsh conditions such as high temperature, high pressure, and chemical corrosion.

Benefits of technology

Amorphous hierarchical porous UiO-66 was successfully prepared at room temperature and normal pressure. It has good biocompatibility and solves the problems of high energy consumption and the use of toxic solvents in traditional methods, laying the foundation for the application of metal-organic framework materials in the biomedical field. Provides new possibilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118063785B_ABST
    Figure CN118063785B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of metal organic framework synthesis, and specifically relates to a method for preparing amorphous multi-level porous UiO-66. The present invention first utilizes ammonium fluoride to promote the dissolution of terephthalic acid in water, and then dissolves zirconium nitrate in water, polyethylene glycol has high hydrophilicity, and its ethoxy repeating unit interacts with zirconium ions, which can promote the coordination self-assembly process of metal ions and organic ligands; zirconium ions and carboxyl groups of terephthalic acid undergo coordination reaction, and this coordination effect is achieved by chemical bonding between zirconium ions and carboxyl oxygen atoms, thereby forming a preliminary coordination polymer structure; as the coordination reaction proceeds, these preliminary coordination polymer structures begin to self-assemble into short-range ordered network structures, and water molecules play the role of a medium in this process, helping zirconium ions and organic ligands to connect in space, thereby preparing amorphous multi-level porous UiO-66.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal organic framework synthesis, and specifically relates to a method for preparing amorphous multi-level porous UiO-66. Background Art

[0002] Metal-organic frameworks (MOFs) are a class of porous materials with high specific surface area, adjustable pore structure and good chemical stability. They are composed of metal ion clusters connected by multi-site organic ligands through coordination bonds. MOFs include crystalline MOFs and amorphous MOFs. Amorphous MOFs exhibit relatively high energy states, have abundant defect sites, and can provide isotropic ion conduction pathways. In recent years, amorphous MOFs have been widely used in reversible gas storage, irreversible long-term storage of hazardous substances, optically active glass and catalysis.

[0003] However, the current synthesis of amorphous MOFs usually requires conditions such as high temperature, high pressure, mechanical ball milling and chemical corrosion to convert crystalline MOFs into amorphous MOFs.

[0004] As a three-dimensional zirconium-based MOFs, UiO-66 has a high specific surface area, thermal stability and chemical stability, and can maintain a crystalline form even when exposed to high external pressure. This excellent stability can be attributed to its strong Zr-O bond and compact cubic close-packed structure. However, this makes the preparation conditions of amorphous UiO-66 more demanding, and it is impossible to prepare amorphous UiO-66 under cell survival conditions, and it cannot be used in the biological field. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing amorphous multi-level porous UiO-66. The preparation method provided by the present invention has mild conditions and can prepare amorphous UiO-66 under cell survival conditions.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing amorphous multi-level porous UiO-66, comprising the following steps:

[0008] (1) first heating and mixing polyethylene glycol, zirconium nitrate and water to obtain a metal solution;

[0009] (2) heating and mixing ammonium fluoride, terephthalic acid and water for a second time to obtain a ligand solution;

[0010] (3) mixing the metal solution and the ligand solution at 15 to 37° C. and normal pressure to carry out coordination reaction to obtain amorphous multi-level porous UiO-66;

[0011] There is no time sequence requirement for step (1) and step (2).

[0012] Preferably, in step (1), the polyethylene glycol is PEG400; the zirconium nitrate is Zr(NO3)4·5H2O; and the water is deionized water.

[0013] Preferably, in step (1), the volume ratio of polyethylene glycol to water is 0.1-10:0.1-10.

[0014] Preferably, in step (1), the mass ratio of water to zirconium nitrate is 0.1-10:0.8-2.5.

[0015] Preferably, the first heating and mixing is stirring and mixing; the temperature of the stirring and mixing is 60 to 90° C., the rotation speed is 500 to 1000 rpm, and the stirring time is 0.5 to 3 hours.

[0016] Preferably, in step (2), the mass ratio of ammonium fluoride to terephthalic acid is 0.5-1.5:0.1-0.3.

[0017] Preferably, in step (2), the mass ratio of ammonium fluoride to water is 0.5 to 1.5:20.

[0018] Preferably, the second heating and mixing is stirring and mixing; the temperature of the stirring and mixing is 60 to 90° C., the rotation speed is 500 to 1000 rpm, and the stirring time is 0.5 to 3 hours.

[0019] Preferably, the molar ratio of the zirconium nitrate to terephthalic acid is 1 to 40:1.

[0020] Preferably, the coordination reaction is carried out under stirring conditions; the stirring speed is 500 to 1000 rpm; and the coordination reaction time is 24 to 72 hours.

[0021] The present invention provides a method for preparing amorphous multi-level porous UiO-66. The present invention first uses ammonium fluoride (NH4F) to promote the dissolution of an organic ligand (terephthalic acid) that is insoluble in water in water, and then dissolves a metal salt (zirconium nitrate) that is easily soluble in water in water. Polyethylene glycol (PEG) has high hydrophilicity, and the ethoxy repeating unit in polyethylene glycol reacts with Zr 4+ The interaction between them can promote the coordination self-assembly process between metal ions and organic ligands, and realize the preparation of amorphous multi-level porous UiO-66 under normal temperature and pressure conditions; in the solution, metal ions (Zr 4+) undergoes a coordination reaction with the carboxyl group of the organic ligand (terephthalic acid). This coordination effect is achieved through the chemical bonding between the metal ions and the carboxyl oxygen atoms, thereby forming a preliminary coordination polymer structure; as the coordination reaction proceeds, these preliminary coordination polymer structures begin to self-assemble into short-range ordered network structures. In this process, water molecules act as a medium, helping the metal ions and organic ligands to connect in space, thereby preparing amorphous multi-level porous UiO-66.

[0022] In the amorphous UiO-66 provided by the present invention, some chemical bonds connecting micropores are in an unconnected state in the amorphous structure, so that the pore size becomes larger, forming mesopores, resulting in the coexistence of mesopores and micropores, that is, the phenomenon of multi-level pores.

[0023] The present invention prepares amorphous multi-level porous UiO-66 at room temperature, normal pressure and in an aqueous phase system, with simple steps, high efficiency and good biocompatibility, and solves the problems of high energy consumption and use of toxic solvents in traditional methods. The present invention provides new possibilities for the application of metal organic framework materials in the biomedical field, especially in aspects such as drug delivery bioimaging and cell therapy. The MOFs material synthesized by the method of the present invention can be more safely applied in vivo, providing a new material basis for research and clinical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 The XRD diffraction pattern comparison diagram of the amorphous UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1;

[0026] Figure 2 A comparison diagram of nitrogen adsorption isotherms of amorphous UiO-66 prepared in Example 1 of the present invention and crystalline UiO-66 prepared in Comparative Example 1;

[0027] Figure 3 The micropore size distribution diagram of the amorphous UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1 (calculated according to the HK method);

[0028] Figure 4 The mesopore size distribution diagram of the amorphous UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1 (calculated according to the BJH desorption branch);

[0029] Figure 5 XRD diagrams of the amorphous multi-level porous UiO-66 prepared in Examples 1 to 3 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1. DETAILED DESCRIPTION

[0030] The present invention provides a method for preparing amorphous multi-level porous UiO-66, comprising the following steps:

[0031] (1) first heating and mixing polyethylene glycol, zirconium nitrate and water to obtain a metal solution;

[0032] (2) heating and mixing ammonium fluoride, terephthalic acid and water for a second time to obtain a ligand solution;

[0033] (3) mixing the metal solution and the ligand solution at 15 to 37° C. and normal pressure to carry out coordination reaction to obtain amorphous multi-level porous UiO-66;

[0034] There is no time sequence requirement for step (1) and step (2).

[0035] In the present invention, polyethylene glycol, zirconium nitrate and water are first heated and mixed to obtain a metal solution. In the present invention, the polyethylene glycol is preferably PEG400; the zirconium nitrate is preferably Zr(NO3)4·5H2O; and the water is preferably deionized water.

[0036] In the present invention, the volume ratio of the polyethylene glycol to water is preferably 0.1-10:0.1-10, more preferably 0.5-8:0.5-8, and further preferably 1-5:1-5.

[0037] In the present invention, the mass ratio of water to zirconium nitrate is preferably 0.1-10:0.8-2.5, more preferably 0.8-8:1.2-2.0, and further preferably 2-5:1.5-1.7.

[0038] In the present invention, the first heating and mixing is preferably: mixing water and polyethylene glycol, and then mixing zirconium nitrate with the obtained mixed solution.

[0039] In the present invention, the first heating mixing is preferably stirring mixing; the temperature of the stirring mixing is preferably 60-90°C, more preferably 70-80°C, further preferably 75°C, the rotation speed is preferably 500-1000rpm, more preferably 600-900rpm, further preferably 700-800rpm, and the stirring time is preferably 0.5-3h, more preferably 1-2.5h, further preferably 1.5-2h.

[0040] In the present invention, the first heating and mixing step preferably further includes cooling the obtained product; the final temperature of the cooling step is preferably room temperature.

[0041] In the present invention, ammonium fluoride, terephthalic acid and water are heated and mixed for a second time to obtain a ligand solution. In the present invention, the water is preferably deionized water.

[0042] In the present invention, the mass ratio of ammonium fluoride to terephthalic acid is preferably 0.5-1.5:0.1-0.3, more preferably 0.7-1.2:0.1-0.3, and further preferably 0.8-1.0:0.2.

[0043] In the present invention, the mass ratio of ammonium fluoride to water is preferably 0.5 to 1.5:20, more preferably 0.7 to 1.2:20, and further preferably 0.9 to 1.1:20.

[0044] In the present invention, the second heating and mixing is preferably: mixing ammonium fluoride with water, and then mixing the obtained mixed solution with terephthalic acid.

[0045] In the present invention, the second heating mixing is preferably stirring mixing; the stirring mixing temperature is preferably 60-90°C, more preferably 70-80°C, further preferably 75°C, the rotation speed is preferably 500-1000rpm, more preferably 600-900rpm, further preferably 700-800rpm, and the stirring time is preferably 0.5-3h, more preferably 1-2.5h, further preferably 1.5-2h.

[0046] In the present invention, the second heating and mixing step preferably further includes cooling the obtained product; the final temperature of the cooling step is preferably room temperature.

[0047] After obtaining the metal solution and the ligand solution, the present invention mixes the metal solution and the ligand solution at 15 to 37° C. and normal pressure conditions to carry out coordination reaction to obtain amorphous multi-level porous UiO-66. In the present invention, the molar ratio of the zirconium nitrate and terephthalic acid is preferably 1 to 40:1, more preferably 7 to 30:1, and further preferably 10 to 20:1.

[0048] In the present invention, the coordination reaction is preferably carried out under stirring conditions; the stirring speed is preferably 500-1000rpm, more preferably 600-900rpm, further preferably 700-800rpm; the coordination reaction time is preferably 24-72h, more preferably 36-60h, further preferably 48h.

[0049] In the present invention, the temperature of the coordination reaction is preferably 18 to 35°C, more preferably 21 to 30°C, and further preferably 24 to 26°C.

[0050] In the present invention, after the coordination reaction, the obtained reaction system is preferably subjected to post-treatment; the post-treatment is preferably: solid-liquid separation of the obtained reaction system, and then sequentially washing, centrifuging, filtering and first drying the obtained solid.

[0051] In the present invention, the solid-liquid separation is preferably centrifugation; the rotation speed of the centrifugation is preferably 1000-5000 rpm, more preferably 2000-4000 rpm, further preferably 3000 rpm, and the time is preferably 5-30 min, more preferably 10-25 min, further preferably 15-20 min.

[0052] In the present invention, the number of washing is preferably 1 to 5 times, more preferably 2 to 4 times, and further preferably 3 times; the washing reagent is preferably an ethanol solution; the volume fraction of the ethanol solution is preferably 95%; the mass volume ratio of the solid to ethanol is preferably 1g:(1 to 3)mL, more preferably 1g:2mL.

[0053] In the present invention, the temperature of the first drying is preferably 60-90° C., more preferably 70-80° C., and the insulation time is preferably 6-24 h, more preferably 10-16 h; and the drying equipment is preferably an oven.

[0054] The present invention removes unreacted substances, impurities or solvent molecules attached to the surface or in the pores of UiO-66 through post-treatment.

[0055] In the present invention, the post-treatment preferably further comprises grinding the obtained solid into powder and then performing a second drying.

[0056] In the present invention, the second drying temperature is preferably 60 to 90° C., more preferably 70 to 80° C., and the heat preservation time is preferably 6 to 24 hours, more preferably 10 to 16 hours.

[0057] The preparation method provided by the present invention can prepare amorphous multi-level porous UiO-66, which has not only a microporous structure but also a mesoporous structure. The micropore diameter is about 0.69 nm and the mesopore diameter is about 3.56 nm.

[0058] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0059] Example 1

[0060] (1) 2.5 mL of deionized water and 2.5 mL of PEG400 solution were fully mixed, and then 0.9193 g of Zr(NO3)4·5H2O was dissolved in the solution. The mixture was stirred at 80°C and 500-1000 r / min for 1 h. After stirring, the mixture was cooled to room temperature to obtain a colorless and transparent metal solution.

[0061] (2) Dissolve 0.765 g of NH4F in 20 mL of deionized water and stir thoroughly to dissolve. Then, dissolve 0.1 g of terephthalic acid in the obtained NH4F solution. Stir at 80°C and 500 r / min for 1 h. After stirring, cool to room temperature to obtain a colorless and transparent ligand solution.

[0062] (3) 5 mL of the ligand solution obtained in step (2) was mixed with the metal solution obtained in step (1), wherein the molar ratio of Zr(NO3)4·5H2O to terephthalic acid was 14.288:1, and the mixture was stirred at 500 r / min at room temperature for 48 h. The obtained product solution was centrifuged at 3000 r / min for 10 min, and the supernatant was removed to obtain a white precipitate.

[0063] (4) The white precipitate obtained in step (3) was washed three times with a 95% by volume ethanol solution, the ratio of the white precipitate to ethanol was 1 g:2 mL, centrifuged, filtered, and dried in an oven at 80° C. for 12 h. The dried solid was ground into powder and vacuum dried at 80° C. for 12 h to obtain amorphous multi-level porous UiO-66, labeled as am-UiO-66-1.

[0064] Example 2

[0065] (1) 5 mL of deionized water and 0.05 mL of PEG400 solution were fully mixed, and then 0.9193 g of Zr(NO3)4·5H2O was dissolved in the solution. The mixture was stirred at 80°C and 500-1000 r / min for 1 h. After stirring, the mixture was cooled to room temperature to obtain a colorless and transparent metal solution.

[0066] (2) Dissolve 0.1 g of NH4F in 20 mL of deionized water and stir thoroughly to dissolve. Then, dissolve 0.036 g of terephthalic acid in the obtained NH4F solution. Stir at 80°C and 500 r / min for 1 h. After stirring, cool to room temperature to obtain a colorless and transparent ligand solution.

[0067] (3) Take 5 mL of the ligand solution obtained in step (2) and mix it with the metal solution obtained in step (1), wherein the molar ratio of Zr(NO3)4·5H2O to terephthalic acid is 40:1, stir at room temperature at 500 r / min for 48 h, centrifuge the obtained product solution at 3000 r / min for 10 min, remove the supernatant, and obtain a white precipitate.

[0068] (4) The white precipitate obtained in step (3) was washed three times with a 95% by volume ethanol solution, the ratio of the white precipitate to ethanol was 1 g:2 mL, centrifuged, filtered, and dried in an oven at 80° C. for 12 h. The dried solid was ground into powder and vacuum dried at 80° C. for 12 h to obtain amorphous multi-level porous UiO-66, labeled as am-UiO-66-2.

[0069] Example 3

[0070] (1) 0.05 mL of deionized water and 5 mL of PEG400 solution were fully mixed, and 0.065 g of Zr(NO3)4·5H2O was dissolved in the solution. The mixture was stirred at 80°C and 500-1000 r / min for 1 h. After stirring, the mixture was cooled to room temperature to obtain a colorless and transparent metal solution.

[0071] (2) Dissolve 0.765 g of NH4F in 20 mL of deionized water and stir thoroughly to dissolve. Then, dissolve 0.1 g of terephthalic acid in the obtained NH4F solution. Stir at 80°C and 500 r / min for 1 h. After stirring, cool to room temperature to obtain a colorless and transparent ligand solution.

[0072] (3) 5 mL of the ligand solution obtained in step (2) was mixed with the metal solution obtained in step (1), wherein the molar ratio of Zr(NO3)4·5H2O to terephthalic acid was 1:1, and the mixture was stirred at 500 r / min at room temperature for 48 h. The obtained product solution was centrifuged at 3000 r / min for 10 min, and the supernatant was removed to obtain a white precipitate.

[0073] (4) The white precipitate obtained in step (3) was washed three times with a 95% by volume ethanol solution, the ratio of the white precipitate to ethanol was 1 g:2 mL, centrifuged, filtered, and dried in an oven at 80° C. for 12 h. The dried solid was ground into powder and vacuum dried at 80° C. for 12 h to obtain amorphous multi-level porous UiO-66, labeled as am-UiO-66-3.

[0074] Comparative Example 1 Traditional Solvothermal Method

[0075] (1) ZrCl4 (0.159 g, 0.68 mmol) and 1,4-terephthalic acid (H2BDC) (0.113 g, 0.68 mmol) were dissolved in DMF (30 mL) at room temperature, respectively. The obtained ZrCl4 solution was then mixed with the 1,4-terephthalic acid solution and transferred to a 50 mL reactor. The mixture was reacted at 120°C for 24 h and crystallized. After cooling, the mixture was centrifuged to obtain a solid precipitate.

[0076] (2) The solid precipitate was washed once with DMF at 40° C., and then the obtained solid was soaked and washed three times with ethanol, and then dried in a vacuum drying oven at 80° C. to obtain crystalline UiO-66, which was labeled as UiO-66-solvent.

[0077] XRD diffraction analysis was performed on the amorphous multi-level porous UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the main peak position and peak intensity of crystalline UiO-66 are consistent with those of standard UiO-66; while the amorphous multi-level porous UiO-66 prepared by the present invention has only three broad "humps" caused by scattering, and the peak intensity is weak, which is a typical feature of amorphous MOFs and can be easily distinguished from crystalline UiO-66; in addition, the crystallinity can also be detected from the peak intensity; according to Figure 1 It can be concluded that the amorphous UiO-66 prepared in Example 1 of the present invention has no obvious crystallization.

[0078] The amorphous multi-level porous UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1 were subjected to nitrogen adsorption isotherm analysis. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the adsorption isotherm of crystalline UiO-66 has an obvious increase in adsorption amount in the low pressure section (relative pressure between 0 and 0.1), and then tends to be flat, which is a typical feature of type I adsorption isotherm, indicating that crystalline UiO-66 is a microporous material; in contrast, the adsorption isotherm of the amorphous UiO-66 provided by the present invention has a significant increase in the low pressure section, and has an obvious hysteresis loop at a relative pressure of 0.4 to 0.7, which is a typical feature of type IV adsorption isotherm, indicating that the amorphous UiO-66 provided by the present invention has a multi-level pore structure.

[0079] The pore size distribution of the amorphous multi-level pore UiO-66 prepared in Example 1 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1 were analyzed. The results are as follows: Figure 3-4 As shown. Figure 3-4 It can be seen that both the amorphous multi-level porous UiO-66 and the crystalline UiO-66 have a microporous structure with pore sizes of 0.69 nm and 0.59 nm, respectively; in addition, the amorphous multi-level porous UiO-66 provided by the present invention has an obvious mesopore distribution at 3.56 nm, indicating that it is a multi-level porous material.

[0080] XRD analysis was performed on the amorphous multi-level porous UiO-66 prepared in Examples 1 to 3 of the present invention and the crystalline UiO-66 prepared in Comparative Example 1. The results are as follows: Figure 5 As shown. Figure 5It can be seen that by changing the ratio of PEG400 to water, and the ratio of zirconium nitrate to terephthalic acid within the protection range, the prepared amorphous multi-level porous UiO-66 has three wide "humps" caused by scattering at the same position, indicating that the present invention has prepared amorphous multi-level porous UiO-66 with a similar structure, indicating that the protection scope of the present invention is desirable.

[0081] It can be seen from the above embodiments that the preparation method provided by the present invention has simple steps, high efficiency and good biocompatibility, which solves the problems of high energy consumption and use of toxic solvents in traditional methods. The amorphous multi-level porous UiO-66 obtained by the present invention provides new possibilities for the application of metal organic framework materials in the biomedical field.

[0082] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing amorphous multi-level porous UiO-66, characterized in that: The following steps are involved: (1) first heating and mixing polyethylene glycol, zirconium nitrate and water to obtain a metal solution; (2) heating and mixing ammonium fluoride, terephthalic acid and water for a second time to obtain a ligand solution; (3) mixing the metal solution and the ligand solution at 15 to 37° C. and normal pressure to carry out coordination reaction to obtain amorphous multi-level porous UiO-66; There is no time sequence requirement for step (1) and step (2); In the step (2), the mass ratio of ammonium fluoride to terephthalic acid is 0.5-1.5:0.1-0.3; the mass ratio of ammonium fluoride to water is 0.5-1.5:20; The molar ratio of the zirconium nitrate to terephthalic acid is 1 to 40:

1.

2. The preparation method according to claim 1, characterized in that: In the step (1), the polyethylene glycol is PEG400; the zirconium nitrate is Zr(NO3)4·5H2O; and the water is deionized water.

3. The preparation method according to claim 1 or 2, characterized in that: In the step (1), the volume ratio of polyethylene glycol to water is 0.1-10:0.1-10.

4. The preparation method according to claim 1 or 2, characterized in that: In the step (1), the mass ratio of water to zirconium nitrate is 0.1-10:0.8-2.

5.

5. The preparation method according to claim 1 or 2, characterized in that: The first heating and mixing is stirring and mixing; the temperature of the stirring and mixing is 60-90° C., the rotation speed is 500-1000 rpm, and the stirring time is 0.5-3 h.

6. The preparation method according to claim 1, characterized in that: The second heating and mixing is stirring and mixing; the stirring and mixing temperature is 60 to 90° C., the rotation speed is 500 to 1000 rpm, and the stirring time is 0.5 to 3 hours.

7. The preparation method according to claim 1, characterized in that: The coordination reaction is carried out under stirring conditions; the stirring speed is 500-1000 rpm; and the coordination reaction time is 24-72 hours.