Recycling treatment method for secondary aluminum ash
By using sodium hydroxide, hydrochloric acid and polyethylene glycol to treat secondary aluminum ash, combined with sodium carbonate roasting and activation, the leaching rate of aluminum elements is improved, and the problem of low resource utilization rate of secondary aluminum ash is solved. Efficient recycling of aluminum and environmental protection.
Patent Information
- Application Number
- PCT/CN2024/073055
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-10
Smart Images

Figure CN2024073055_10102024_PF_FP_ABST
Abstract
Description
A resource processing method for secondary aluminum ash Technical Field
[0001] The present invention belongs to the technical field of solid waste resource treatment, and specifically relates to a resource treatment method for secondary aluminum ash. Background Art
[0002] Aluminum ash is a solid waste generated during aluminum electrolysis, aluminum processing, and aluminum recycling. It can be divided into primary and secondary aluminum ash. Aluminum shavings, aluminum slag, and other aluminum-containing wastes are directly generated during the electrolysis, processing, and recycling processes. These wastes are collectively referred to as primary aluminum ash. Primary aluminum ash contains over 30% metallic aluminum. The slag obtained after treatments such as roasting, pressing, or rotary kiln processing is called secondary aluminum ash. Because it contains small amounts of toxic substances such as heavy metals and fluorides, it is classified as hazardous waste. With the rapid development of the electrolytic aluminum industry, the annual output of aluminum ash is significant, necessitating the efficient and effective recovery and comprehensive utilization of aluminum ash.
[0003] Aluminum ash processing typically involves two steps: the first is the extraction of primary aluminum ash, which contains 15% to 75% Al by mass and is typically off-white, also known as "white aluminum ash." Metallic aluminum is often extracted through methods such as ash roasting. The roasting method involves adding the aluminum ash and a certain amount of salt flux to an iron pan. Heat is generated by the ash's own oxidation, and the ash is stirred with a shovel. Simultaneously, the magnesium and other substances in the ash continue to oxidize and release heat, melting the metallic aluminum and pooling at the bottom of the pan. The molten aluminum can then flow out and be recovered. The second step is the extraction of secondary aluminum ash, which contains approximately 7% to 30% Al and is typically gray-black, also known as "black aluminum ash." This ash has a low aluminum content and a complex composition, making it difficult to process. Therefore, traditional disposal methods often involve landfilling or disposal. However, the hazardous properties of secondary aluminum ash include reactivity (R) and toxicity (T). Direct landfilling or disposal poses environmental risks and fails to effectively utilize the valuable aluminum.
[0004] Patent CN 111233003 A discloses an acid-base combined process for fully realizing resource utilization of high-fluorine secondary aluminum ash. The process includes the following steps: ball milling the high-fluorine secondary aluminum ash, screening to remove metallic aluminum, and then dividing it into two parts; one part is first water-leached and then acid-leached, followed by solid-liquid separation to obtain an acid leaching solution and an acid leaching residue; the other part is mixed with an alkaline solution, alkaline-leached, and then solid-liquid separation to obtain an alkaline leaching solution and an alkaline leaching residue; the acid leaching solution and the alkaline leaching solution are mixed in proportion to a pH value close to neutral, stirred, filtered, and the solid is dried and then roasted for dehydration to obtain an electrolyte product, and the filtrate is returned to the ball milling process. This patent mainly uses leaching to convert nitrogen, fluorine, sodium, and aluminum leached from the electrolytic aluminum ash into ammonia water and an electrolyte product, while also obtaining high-purity alumina (i.e., acid leaching residue and alkaline leaching residue), which can be used as raw materials to prepare products such as high-alumina bricks and refractory materials. Patent CN 112266063 A discloses a method for preparing a polyaluminum chloride water purifier from secondary aluminum ash from recycled aluminum. The method involves screening, washing, filtering, acid leaching, suction filtration, and polymerization and aging to produce a liquid polyaluminum chloride product. Patent CN 109761323 A discloses a method for preparing a water purifier containing polyaluminum chloride from aluminum ash, hydrochloric acid, and optionally red mud. The method comprises the following steps: mixing the aluminum ash with sodium carbonate and / or sodium hydroxide and a calcium-containing raw material; calcining the calcined product at 400-1000°C in an oxidizing atmosphere; reacting the calcined product with hydrochloric acid and optionally red mud; and filtering the resulting product to produce a water purifier containing polyaluminum chloride.
[0005] Although the above-mentioned prior art discloses resource utilization of aluminum element in secondary aluminum ash, its resource utilization rate needs to be further improved. Summary of the Invention
[0006] In view of the shortcomings and deficiencies of the above-mentioned prior art, the present invention aims to provide a method for resource recovery of secondary aluminum ash, which can significantly improve the leaching and resource utilization rate of Al in secondary aluminum ash.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for recycling secondary aluminum ash, comprising the following steps:
[0009] (1) mixing secondary aluminum ash with sodium hydroxide solution, heating for leaching, and filtering to obtain leachate and filter residue, and drying the filter residue to obtain alkaline leaching residue;
[0010] (2) mixing the alkaline leaching residue obtained in step (1) with a hydrochloric acid solution, heating and leaching, then adding polyethylene glycol and stirring and mixing uniformly, filtering to obtain a leachate and a filter residue, and drying the filter residue to obtain an acid leaching residue;
[0011] (3) mixing the acid leaching residue obtained in step (2) with sodium carbonate, and then performing a roasting activation treatment at a temperature of 800 to 900° C. to obtain roasted residue;
[0012] (4) subjecting the roasted slag obtained in step (3) to acid leaching, water leaching or alkaline leaching, and filtering to obtain a leachate and residual solid slag.
[0013] Furthermore, the mass ratio of the secondary aluminum ash to the sodium hydroxide added in step (1) is 50:3 to 10:1.
[0014] Furthermore, the liquid-to-solid ratio (ml / g) of the secondary aluminum ash mixed with the sodium hydroxide solution in step (1) is 3:1 to 6:1.
[0015] Furthermore, the temperature of the heating leaching in step (1) is 80-100° C., and the time is 3-4 hours.
[0016] Furthermore, in step (2), the liquid-to-solid ratio (ml / g) of the alkali leaching residue mixed with the hydrochloric acid solution is 3:1 to 6:1.
[0017] Furthermore, the temperature of the heating leaching in step (2) is 80-100° C., and the time is 3-5 hours.
[0018] Furthermore, the amount of polyethylene glycol added in step (2) is 1% to 5% of the mass of the alkali leaching residue.
[0019] Furthermore, the mass ratio of the acid leaching residue and sodium carbonate mixed in step (3) is 1:1 to 5:1.
[0020] Furthermore, the time for the calcination activation treatment in step (3) is 2 to 4 hours.
[0021] Furthermore, the leachate obtained in steps (1), (2) and (4) is used as a raw material for preparing a polyaluminium chloride water purifier.
[0022] The principle of the present invention is:
[0023] First, a large amount of AlN in the secondary aluminum ash is removed by alkaline leaching. The Al in the remaining residue mainly exists in the form of corundum, magnesia-alumina spinel, a small amount of AlN, metallic Al, etc. These substances can react with HCl solution to produce AlCl 3 solution. The main leaching reactions are as follows:
[0024] AlN+NaOH+H 2 O=NaAlO 2 +NH 3 ↑ (1)
[0025] 2Al+6HCl=2AlCl 3 +3H 2 ↑ (2)
[0026] Al 2 O 3 +6HCl=2AlCl 3 +3H 2 O (3)
[0027] AlN+4HCl=AlCl 3 +NH 4 Cl (4)
[0028] Acid leaching extracts nitrogen and the more easily leached aluminum from the secondary aluminum ash, producing an acid leaching residue. The added polyethylene glycol acts as a flocculant, producing some aluminum chloride colloid in the solution after acid leaching. The addition of polyethylene glycol as a flocculant facilitates the post-leaching filtration process by stirring. The secondary aluminum ash acid leaching residue is then roasted with sodium carbonate salt. The high-temperature activation of the sodium salt breaks down the hard structures of the corundum and other materials in the residue, thereby increasing the leaching rate of the aluminum in the acid leaching residue and further utilizing it as a resource.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The method of the present invention obtains a polyaluminium chloride solution through alkaline leaching, acid leaching, roasting activation and leaching, which can be used in the fields of drinking water, industrial water and sewage treatment to achieve the recycling of aluminium in aluminium ash, thereby reducing the pollution and harm to the environment caused by the storage of aluminium ash and alleviating the pressure on bauxite resources.
[0031] (2) The present invention solves the problem that the main component of aluminum ash, aluminum oxide (corundum), cannot be utilized due to its poor activity and causes great waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is an appearance diagram of the secondary aluminum ash original sample (a) and the secondary aluminum ash acid leaching residue (b) and roasting slag sample (c) obtained after leaching in Example 1 of the present invention.
[0033] FIG2 is an XRD diagram of the secondary aluminum ash original sample (a) and the secondary aluminum ash acid leaching residue (b) and roasting residue sample (c) obtained after leaching in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The present invention will be described in further detail below with reference to the embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0035] Comparative Example 1
[0036] A secondary aluminum ash sample was alkaline-leached with sodium hydroxide solution at 90°C for 3 hours at a liquid-to-solid ratio (ml / g) of 3:1. The secondary aluminum ash and sodium hydroxide were added at a mass ratio of 20:1. The sample was filtered and dried. The alkaline-leached residue was stirred and leached with 6M HCl at a liquid-to-solid ratio of 3:1 at 90°C for 3 hours. The residue was then filtered and dried at 70°C to obtain a secondary aluminum ash acid-leached residue. 1g of the secondary aluminum ash acid-leached residue was then leached with 20ml of deionized water to obtain a leachate. The Al 3+ concentration in the leachate was determined using ICP. In this comparative example, 10g of secondary aluminum ash was treated, and the Al 3+ concentration in the leachate was determined to be 439.24mg / L. The calculated Al leaching mass concentration in the acid-leached residue was 8.79mg / g.
[0037] Example 1
[0038] A secondary aluminum ash sample was alkaline-leached with sodium hydroxide solution at 90°C for 3 hours at a liquid-to-solid ratio (ml / g) of 3:1. The secondary aluminum ash and sodium hydroxide were added at a mass ratio of 20:1. The sample was filtered and dried. The alkaline-leached residue was stirred and leached with 6M HCl at a liquid-to-solid ratio of 3:1 at 90°C for 3 hours. The residue was then filtered and dried at 70°C to obtain a secondary aluminum ash acid-leached residue. The secondary aluminum ash acid-leached residue was then mixed with sodium carbonate at a ratio of 1:1 and calcined at 800°C for 3 hours to obtain a calcined residue sample. One gram of the calcined residue sample was then leached with 20 ml of deionized water to obtain a leachate. The Al⁺ ...
[0039] By comparing the results with those of Comparative Example 1, it can be seen that the present invention improves the leaching of Al in the secondary aluminum ash acid leaching residue by adding sodium carbonate to the secondary aluminum ash acid leaching residue for roasting and activation treatment.
[0040] Figure 1 shows the appearance of the secondary aluminum ash sample treated in this example, as well as the secondary aluminum ash acid leaching residue and calcined slag samples obtained after leaching. Figure 1 shows that the secondary aluminum ash acid leaching residue is a gray-black powder, while the calcined slag is a yellow-white powder. Figure 2 shows the XRD patterns of the secondary aluminum ash sample before treatment and the secondary aluminum ash acid leaching residue and calcined slag samples obtained after leaching. Figure 2 shows that the primary components of the secondary aluminum ash acid leaching residue sample are alumina and magnesia-alumina spinel, while the primary components of the calcined slag sample are magnesia-alumina spinel. This further demonstrates that sodium carbonate roasting and activation treatment can break down the hard structure of alumina, such as corundum.
[0041] Example 2
[0042] A secondary aluminum ash sample was alkaline-leached at 80°C for 4 hours with a sodium hydroxide solution at a liquid-to-solid ratio (ml / g) of 4:1. The secondary aluminum ash was added at a mass ratio of 10:1. The sample was then filtered and dried. The alkaline-leached residue was stirred and leached at 80°C for 5 hours with 6M HCl at a liquid-to-solid ratio of 4:1. The residue was then filtered and dried at 70°C to obtain a secondary aluminum ash acid-leached residue. The secondary aluminum ash acid-leached residue was then mixed with sodium carbonate at a ratio of 2:1 and calcined at 900°C for 2 hours to obtain a calcined residue sample. One gram of the calcined residue sample was then leached with 20 ml of hydrochloric acid solution to obtain a leachate. The Al 3+ concentration in the leachate was determined to be 1210.24 mg / L, and the calculated Al leached mass concentration in the calcined residue sample was 24.20 mg / g.
[0043] Example 3
[0044] A secondary aluminum ash sample was alkaline-leached with sodium hydroxide solution at 100°C for 3 hours at a liquid-to-solid ratio (ml / g) of 5:1. The secondary aluminum ash was added at a mass ratio of 40:1. The sample was filtered and dried. The alkaline-leached residue was stirred and leached with 6M HCl at a liquid-to-solid ratio of 5:1 at 100°C for 3 hours. The residue was then filtered and dried at 70°C to obtain a secondary aluminum ash acid-leached residue. The secondary aluminum ash acid-leached residue was then mixed with sodium carbonate at a ratio of 3:1 and calcined at 800°C for 4 hours to obtain a calcined residue sample. One gram of the calcined residue sample was then leached with 20 ml of sodium hydroxide solution to obtain a leachate. The Al 3+ concentration in the leachate was determined to be 1157.68 mg / L, and the calculated Al leached mass concentration in the calcined residue sample was 23.15 mg / g.
[0045] The above embodiments are preferred implementations of the present invention, but the implementations of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.
Claims
1. A method for recycling secondary aluminum ash, characterized in that: The steps include: (1) mixing secondary aluminum ash with sodium hydroxide solution, heating for leaching, and filtering to obtain leachate and filter residue, and drying the filter residue to obtain alkaline leaching residue; (2) mixing the alkaline leaching residue obtained in step (1) with a hydrochloric acid solution, heating and leaching, then adding polyethylene glycol and stirring and mixing uniformly, filtering to obtain a leachate and a filter residue, and drying the filter residue to obtain an acid leaching residue; (3) mixing the acid leaching residue obtained in step (2) with sodium carbonate, and then performing a roasting activation treatment at a temperature of 800 to 900° C. to obtain roasted residue; (4) subjecting the roasted slag obtained in step (3) to acid leaching, water leaching or alkaline leaching, and filtering to obtain a leachate and residual solid slag.
2. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The mass ratio of the secondary aluminum ash to the sodium hydroxide added in step (1) is 50:3 to 10:
1.
3. The resource recovery method of secondary aluminum ash according to claim 1, characterized in that: The liquid-to-solid ratio of the secondary aluminum ash and the sodium hydroxide solution in step (1) is 3:1 to 6:
1.
4. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The heating leaching temperature in step (1) is 80-100° C. and the time is 3-4 hours.
5. The resource recovery method of secondary aluminum ash according to claim 1, characterized in that: The liquid-to-solid ratio of the alkali leaching residue and the hydrochloric acid solution in step (2) is 3:1 to 6:
1.
6. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The heating leaching in step (2) is carried out at a temperature of 80 to 100° C. and for a time of 3 to 5 hours.
7. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The amount of polyethylene glycol added in step (2) is 1% to 5% of the mass of the alkali leaching residue.
8. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The mass ratio of the acid leaching residue and sodium carbonate mixed in step (3) is 1:1 to 5:
1.
9. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The time of the calcination activation treatment in step (3) is 2 to 4 hours.
10. The method for recycling secondary aluminum ash according to claim 1, characterized in that: The leachate obtained in steps (1), (2) and (4) is used as a raw material for preparing a polyaluminium chloride water purifier.
Citation Information
Patent Citations
Resource utilization method of aluminum ash
CN103555955A
Method for preparing aluminum-silicon oxide from fly ash
CN111606339A
Method for treating secondary aluminum ash through dry ternary roasting
CN113149034A
Aluminum ash resource utilization method
CN113479920A
Method for co-processing and resource utilization of aluminum ash and household garbage incineration fly ash
CN114182103A
Cited By
High-thermal-shock insulating brick based on aluminum ash and preparation method of high-thermal-shock insulating brick
CN119569430A
Method for recovering aluminum in electrolytic aluminum ash
CN121046651A
Combined treatment method for aluminum ash and waste aluminum electrolyte
CN121426152A
Method for treating secondary aluminum ash based on two-step pyrogenic process calcination
CN121776227A