A two-dimensional polyamide-modified polyimide composite material and preparation method thereof
By uniformly dispersing two-dimensional polyamide in polyimide and preparing composite materials using ultrasonic assisted dispersion and thermoforming processes, the problem of insufficient barrier performance of polyimide films is solved, and the mechanical properties of the material are improved and significant barrier properties are achieved. Improved, suitable for FOLED and other fields.
Patent Information
- Application Number
- CN202410152477.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-02-03
AI Technical Summary
The existing polyimide films have poor barrier properties to water vapor and oxygen, and the nano-layered fillers have poor compatibility with polyimides, making the process difficult to control, which limits their application in electronic equipment.
Using a composite material of two-dimensional polyamide (2DPA) and polyimide (PI), 2DPA is uniformly dispersed in PI through π-π conjugation and interlayer hydrogen bonding, and ultrasonic assisted dispersion and thermoforming processes are used to prepare the Composite material with excellent barrier properties.
It significantly improves the mechanical properties and barrier properties of polyimide materials, providing new directions and application prospects for high barrier materials, especially in the fields of FOLED and portable smart electronic products.
Smart Images

Figure BDA0004696187060000031 
Figure FDA0005007637770000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer composite materials, and in particular to a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof. Background Art
[0002] Polyimide is a polymer material with excellent heat resistance and high strength. It also has the advantages of low dielectric constant, high insulation, and small thermal expansion. It is widely used in aerospace, electronics, precision instruments, automobile manufacturing and other fields.
[0003] The poor barrier properties of polyimide films to water vapor and oxygen limit their application in electronic devices, such as flexible organic light-emitting devices (FOLEDs). In recent years, researchers have prepared a variety of nano-layered filler-modified polyimide composites, which have significantly improved barrier properties compared to pure polyimide films. However, since the nano-layered fillers currently used are all inorganic, they have poor compatibility with polyimide, are easy to agglomerate, and the process is difficult to control. In addition, the nano-layered fillers need to be acidified, ion-exchanged, cleaned, and the process cycle is long.
[0004] According to the Nieslen model, adding layered materials to polyimide is conducive to forming a "tortuous path" to extend the permeation path of small molecules and hinder the diffusion of small molecules in the matrix, thereby significantly improving the barrier properties of the material. Recently, the literature reported the successful preparation of a two-dimensional polyamide (2DPA), which has excellent mechanical strength and ultra-high barrier properties. The present invention uniformly disperses 2DPA in a polyimide substrate through π-π conjugation and interlayer hydrogen bonding, achieves effective interfacial contact and strong interfacial bonding between layers, and successfully prepares a new type of two-dimensional polyamide / polyimide composite material, which can effectively improve the mechanical properties and barrier properties of polyimide materials. The present invention provides a new direction and new ideas for the preparation of high-barrier materials, and has application prospects in the fields of FOLED flexible display devices, portable smart electronic products, battery separators, etc. Summary of the invention
[0005] The methods reported by predecessors to improve the barrier properties of PI are almost all to add inorganic fillers. Such methods can effectively improve its barrier properties, but inorganic fillers also have the disadvantages of poor compatibility with polyimide, easy agglomeration, and difficult process control. In order to make up for this deficiency, the present invention uses organic layered material polyamide as filler to provide a method for preparing a two-dimensional polyamide-modified polyimide composite material.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, characterized in that: a certain amount of 2DPA, diamine and dianhydride are dissolved in a solvent in a certain proportion, 2DPA is dispersed with the aid of ultrasound, and stirred for a certain time at a certain temperature and atmosphere to finally obtain a 2DPA / PAA solution. The 2DPA / PAA solution is then scraped onto a substrate and subjected to a thermoforming process to obtain a 2DPA / PI composite material.
[0008] According to the present invention, the two-dimensional polyamide has a structure shown in Formula 1, and its repeating unit molecule includes triamine substituted unsaturated six-membered ring A and triacyl chloride substituted unsaturated six-membered ring B. The overall structure contains an amide group, a benzene ring, and a triazine ring.
[0009]
[0010] According to the present invention, the size of 2DPA is about 100 to 200 nm, and the microscopic shape is a layered stack.
[0011] According to the present invention, the mass ratio of 2DPA to PAA is 0.5% to 10%.
[0012] The present invention is characterized in that the dianhydride monomer is at least one of pyromellitic dianhydride, 3,3',4,4'benzophenone tetracarboxylic dianhydride, 4,4'biphenyl ether dianhydride, 4,4'[hexafluoroisopropyl]diphthalic anhydride, 3,3',4,4'biphenyltetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, cyclobutanetetracarboxylic dianhydride, and bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, or a derivative thereof.
[0013] In the present invention, the diamine monomer is at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 1,4-cyclohexanediamine, p-phenylenediamine, 4,4'-diaminobenzanilide, 2,2'-bis(trifluoromethyl)diaminobiphenyl, or a derivative thereof.
[0014] According to the present invention, the molar ratio of dianhydride to diamine is 0.95 to 1.1.
[0015] According to the present invention, the solvent is at least one of N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide or N,N-diethylformamide.
[0016] 9. According to the present invention, the time of ultrasound-assisted dispersion is 1 to 5 hours.
[0017] According to the present invention, the stirring reaction temperature is 0-40° C., the atmosphere is nitrogen or other inert gases, and the stirring time is 10-16 hours.
[0018] In the 2DPA / polyamic acid (PAA) solution of the present invention, the mass ratio of polyamic acid to solvent is 10% to 20%.
[0019] In the present invention, the substrate is one of a glass substrate, a marble substrate and a silicon wafer substrate.
[0020] According to the present invention, the hot forming process is programmed heating, the heating temperature range is 30 to 400° C., and the insulation time of each temperature section is 30 to 100 minutes. DETAILED DESCRIPTION
[0021] For the convenience of understanding the present invention, the present invention enumerates the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. The technical scheme in the present invention will be clearly and completely described below in conjunction with the embodiments in the present invention.
[0022] Example 1
[0023] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 4,4' diaminodiphenyl ether, and pyromellitic dianhydride;
[0024] The preparation method comprises the following steps:
[0025] 5 wt% 2DPA was added, 4,4'-diaminodiphenyl ether and pyromellitic anhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:95, 2DPA was dispersed with ultrasound assistance for 2 h, and stirred at 25 °C in a nitrogen atmosphere for 10 h to obtain a 15 wt% 2DPA / PAA solution (2DPA:PAA=5 wt%).
[0026] A 15wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 120°C → 150°C → 200°C → 250°C → 300°C → 350°C, with each temperature section being kept for 1 hour to obtain a 2DPA / PI composite material (2DPA: PI = 5wt%).
[0027] Example 2
[0028] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 4,4' diaminodiphenylmethane, 3,3',4,4' dibenzophenone tetracarboxylic dianhydride;
[0029] The preparation method comprises the following steps:
[0030] 0.5 wt% 2DPA was added, 4,4' diaminodiphenylmethane and 3,3',4,4' dibenzophenonetetracarboxylic dianhydride were dissolved in N-methyl-2-pyrrolidone at a ratio of 100:98, 2DPA was dispersed with the aid of ultrasound for 3 h, and stirred at 20 °C in a nitrogen atmosphere for 12 h to obtain a 10 wt% 2DPA / PAA solution (2DPA:PAA=0.5 wt%).
[0031] A 10wt% 2DPA / PAA solution was scraped onto a marble substrate and subjected to a thermoforming process: uniform heating of 30°C → 120°C → 150°C → 200°C → 250°C → 300°C → 350°C → 400°C, with each temperature section being kept warm for 30 min to obtain a 2DPA / PI composite material (2DPA: PI = 0.5wt%).
[0032] Example 3
[0033] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 1,4-cyclohexanediamine, 4,4'-biphenyl ether dianhydride;
[0034] The preparation method comprises the following steps:
[0035] 2 wt% 2DPA was added, 1,4-cyclohexanediamine and 4,4'-biphenyl ether dianhydride were dissolved in N-ethyl-2-pyrrolidone at a ratio of 100:105, 2DPA was dispersed with ultrasound assistance for 1 h, and stirred at 30°C in a nitrogen atmosphere for 14 h to obtain a 12 wt% 2DPA / PAA solution (2DPA:PAA=2 wt%).
[0036] A 12wt% 2DPA / PAA solution was scraped onto a silicon wafer substrate and subjected to a thermal forming process: uniform heating of 30°C → 70°C → 100°C → 150°C → 200°C → 250°C → 300°C → 350°C, with each temperature section being kept for 40 minutes to obtain a 2DPA / PI composite material (2DPA: PI = 2wt%).
[0037] Example 4
[0038] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, p-phenylenediamine, 4,4′[hexafluoroisopropyl]diphthalic anhydride;
[0039] The preparation method comprises the following steps:
[0040] 4 wt% 2DPA was added, p-phenylenediamine and 4,4′[hexafluoroisopropyl]diphthalic anhydride were dissolved in N,N-dimethylformamide at a ratio of 100:110, 2DPA was dispersed with the aid of ultrasound for 5 h, and stirred at 40°C in a nitrogen atmosphere for 16 h to obtain a 20 wt% 2DPA / PAA solution (2DPA:PAA=4 wt%).
[0041] A 20wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 150°C → 200°C → 250°C → 300°C → 350°C, with each temperature section being kept warm for 100 min to obtain a 2DPA / PI composite material (2DPA: PI = 4wt%).
[0042] Example 5
[0043] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 4,4' diaminodiphenyl ether, 3,3',4,4' biphenyltetracarboxylic dianhydride;
[0044] The preparation method comprises the following steps:
[0045] Add 6 wt% 2DPA, dissolve 4,4' diaminodiphenyl ether and 3,3',4,4' biphenyltetracarboxylic dianhydride in N,N-diethylformamide at a ratio of 100:102, disperse 2DPA with the aid of ultrasound for 4 h, stir at 10°C in a nitrogen atmosphere for 11 h to obtain an 18 wt% 2DPA / PAA solution (2DPA:PAA=6 wt%).
[0046] An 18wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 120°C → 150°C → 200°C → 250°C → 300°C, with each temperature section being kept warm for 80 minutes to obtain a 2DPA / PI composite material (2DPA: PI = 6wt%).
[0047] Example 6
[0048] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 2,2'-bis(trifluoromethyl)diaminobiphenyl, and 1,4,5,8-naphthalenetetracarboxylic anhydride;
[0049] The preparation method comprises the following steps:
[0050] 8 wt% 2DPA was added, 2,2'-bis(trifluoromethyl)diaminobiphenyl and 1,4,5,8-naphthalenetetracarboxylic anhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:96, 2DPA was dispersed with the aid of ultrasound for 5 h, and stirred at 35 °C in a helium atmosphere for 13 h to obtain a 16 wt% 2DPA / PAA solution (2DPA:PAA=8 wt%).
[0051] A 16wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 100°C → 120°C → 150°C → 250°C → 350°C, with each temperature section being kept warm for 70 min to obtain a 2DPA / PI composite material (2DPA: PI = 8wt%).
[0052] Example 7
[0053] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 4,4'-diaminobenzanilide, 1,2,4,5-cyclohexanetetracarboxylic dianhydride;
[0054] The preparation method comprises the following steps:
[0055] 10 wt% 2DPA was added, 4,4'-diaminobenzanilide and 1,2,4,5-cyclohexanetetracarboxylic dianhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:97, 2DPA was dispersed with ultrasound assistance for 3 h, and stirred at 5 °C in a nitrogen atmosphere for 14 h to obtain a 17 wt% 2DPA / PAA solution (2DPA:PAA=10 wt%).
[0056] A 17wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 120°C → 150°C → 250°C → 350°C → 400°C, with each temperature section being kept warm for 40 minutes to obtain a 2DPA / PI composite material (2DPA: PI = 10wt%).
[0057] Example 8
[0058] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 1,4-cyclohexanediamine, and cyclobutanetetracarboxylic dianhydride;
[0059] The preparation method comprises the following steps:
[0060] 0.8 wt% of 2DPA was added, 1,4-cyclohexanediamine and cyclobutanetetracarboxylic dianhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:102, 2DPA was dispersed with the aid of ultrasound for 2 h, and stirred at 25 °C in an argon atmosphere for 10 h to obtain a 14 wt% 2DPA / PAA solution (2DPA:PAA=0.8 wt%).
[0061] A 14wt% 2DPA / PAA solution was scraped onto a silicon wafer substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 100°C → 150°C → 250°C → 300°C → 350°C, with each temperature section being kept for 50 min to obtain a 2DPA / PI composite material (2DPA: PI = 0.8wt%).
[0062] Example 9
[0063] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, p-phenylenediamine, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride;
[0064] The preparation method comprises the following steps:
[0065] Add 3 wt% 2DPA, dissolve p-phenylenediamine and bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride in N,N-dimethylacetamide at a ratio of 100:96, disperse 2DPA with the assistance of ultrasound for 2 h, stir at 0°C and nitrogen atmosphere for 10 h to obtain a 13 wt% 2DPA / PAA solution (2DPA:PAA=3 wt%).
[0066] A 13wt% 2DPA / PAA solution was scraped onto a marble substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 100°C → 150°C → 250°C → 300°C, with each temperature section being kept for 90 minutes to obtain a 2DPA / PI composite material (2DPA: PI = 3wt%).
[0067] Example 10
[0068] This embodiment provides a two-dimensional polyamide-modified polyimide composite material and a preparation method thereof, wherein the composite material comprises the following components: 2DPA, 4,4'-diaminobenzanilide, and pyromellitic dianhydride;
[0069] The preparation method comprises the following steps:
[0070] 5 wt% 2DPA was added, 4,4'-diaminobenzanilide and pyromellitic anhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:100, 2DPA was dispersed with ultrasound assistance for 3 h, and stirred at 25 °C in a nitrogen atmosphere for 12 h to obtain a 12 wt% 2DPA / PAA solution (2DPA:PAA=5 wt%).
[0071] A 12wt% 2DPA / PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 100°C → 150°C → 250°C → 300°C → 350°C → 400°C, with each temperature section being kept warm for 1h to obtain a 2DPA / PI composite material (2DPA: PI = 5wt%).
[0072] Comparative Example 1 does not contain 2DPA.
[0073] This comparative example provides a polyimide material and a preparation method thereof, wherein the material comprises the following components: 4,4' diaminodiphenyl ether, pyromellitic dianhydride;
[0074] The preparation method comprises the following steps:
[0075] 4,4'-diaminodiphenyl ether and pyromellitic anhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:95, and stirred at 25°C under a nitrogen atmosphere for 10 hours to obtain a 15 wt% PAA solution.
[0076] A 15wt% PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 120°C → 150°C → 200°C → 250°C → 300°C → 350°C, with each temperature section being kept for 1 hour to obtain a polyimide material.
[0077] Comparative Example 2 does not contain 2DPA compared to Example 10.
[0078] This comparative example provides a polyimide material and a preparation method thereof, wherein the material comprises the following components: 4,4'-diaminobenzanilide, pyromellitic dianhydride;
[0079] The preparation method comprises the following steps:
[0080] 4,4'-Diaminobenzanilide and pyromellitic anhydride were dissolved in N,N-dimethylacetamide at a ratio of 100:100, and stirred at 25°C under a nitrogen atmosphere for 12 hours to obtain a 12 wt% PAA solution.
[0081] A 12wt% PAA solution was scraped onto a glass substrate and subjected to a thermoforming process: uniform heating of 30°C → 70°C → 100°C → 150°C → 250°C → 300°C → 350°C → 400°C, with each temperature section being kept for 1 hour to obtain a 2DPA / PI composite material.
[0082] Implementation effect example
[0083] 1. Oxygen permeability of polyimide materials of Examples 1-10 and Comparative Examples 1-2
[0084] The oxygen permeability of the polyimide material was measured according to the standard GB / T 1038-2022 Test method for gas permeability of plastic films and sheets, as shown in Table 1.
[0085] Table 1 Oxygen permeability of different polyimide materials
[0086] sample <![CDATA[Oxygen transmission rate cm 3 / (m 2 ·24h·0.1MPa)]]> Example 1 181.32 Example 2 45.42 Example 3 14.78 Example 4 25.26 Example 5 39.88 Example 6 9.26 Example 7 20.19 Example 8 32.59 Example 9 9.52 Example 10 1.72 Comparative Example 1 657.34 Comparative Example 2 7.92
[0087] II. Moisture Permeability of Polyimide Materials in Examples 1-10 and Comparative Examples 1-2
[0088] The moisture permeability of the polyimide material was measured according to the standard GB / T 1037-2021 Test method for water vapor permeability of plastic films and sheets, as shown in Table 2.
[0089] Table 2 Water vapor transmission rate of different polyimide materials
[0090] sample <![CDATA[Water vapor transmission rate g / (m 2 ·24h·0.1MPa)]]> Example 1 108.42 Example 2 45.26 Example 3 35.21 Example 4 13.14 Example 5 40.24 Example 6 24.15 Example 7 35.68 Example 8 34.02 Example 9 22.43 Example 10 1.23 Comparative Example 1 209.79 Comparative Example 2 5.04
[0091] The applicant declares that the above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a two-dimensional polyamide-modified polyimide composite material, characterized in that: The preparation method comprises the following steps: Putting 2DPA, diamine monomer and dianhydride monomer into an organic solvent and dispersing the 2DPA with the aid of ultrasound, reacting in an inert gas atmosphere and under stirring to obtain a 2DPA / PAA solution, wherein the mass ratio of 2DPA to PAA in the 2DPA / PAA solution is 0.5% to 10%, and the temperature is controlled at 0 to 40° C. during the reaction; Then, the 2DPA / PAA solution is scraped onto the substrate, and then the two-dimensional polyamide-modified polyimide composite material is obtained by thermoforming; The 2DPA has a structure as shown in Formula 1: The repeating unit molecule of the 2DPA includes a triamine-substituted unsaturated six-membered ring A and a triacyl chloride-substituted unsaturated six-membered ring B. The overall structure of the 2DPA contains an amide group, a benzene ring, and a triazine ring. The size of the 2DPA is 100 to 200 nm, and the microscopic shape of the 2DPA is a layered stack. The molar ratio of the dianhydride to the diamine is 0.95 to 1.1; The dianhydride monomer is at least one of pyromellitic dianhydride, 3,3',4,4'benzophenone tetracarboxylic dianhydride, 4,4'biphenyl ether dianhydride, 4,4'[hexafluoroisopropyl]diphthalic anhydride, 3,3',4,4'biphenyltetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic anhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, cyclobutane tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, or a derivative thereof; The diamine monomer is at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 1,4-cyclohexanediamine, p-phenylenediamine, 4,4'-diaminobenzanilide, 2,2'-bis(trifluoromethyl)diaminobiphenyl, or a derivative thereof.
2. The preparation method according to claim 1, characterized in that: The organic solvent is at least one of N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide or N,N-diethylformamide.
3. The preparation method according to claim 1, characterized in that: The ultrasonic-assisted dispersion time is 1 to 5 hours, the inert gas is nitrogen, and the stirring time is 10 to 16 hours.
4. The preparation method according to claim 1, characterized in that: The mass ratio of PAA to the organic solvent in the 2DPA / PAA solution is 10% to 20%.
5. The preparation method according to claim 1, characterized in that: The substrate is a glass substrate, a marble substrate or a silicon wafer substrate.
6. The preparation method according to claim 1, characterized in that: The thermoforming process is programmed heating, the heating temperature range is 30 to 400°C, and the insulation time in each temperature section is 30 to 100 minutes.
7. A two-dimensional polyamide-modified polyimide composite material, characterized in that: The preparation method is described in any one of claims 1 to 6.
Citation Information
Patent Citations
Water / oxygen barrier polymer-based composite material as well as preparation method and application thereof
CN106750438A
Anticorrosive dispersion liquid and preparation method thereof
CN117363069A