A method for controlling the deformation heat treatment of TaC in CLAM steel

By controlling the deformation heat treatment method of TaC in CLAM steel, the problem of insufficient high-temperature mechanical properties of CLAM steel was solved, and the high-temperature performance was significantly improved, meeting the performance requirements of fusion reactor blanket structure materials.

CN118064690BActive Publication Date: 2026-11-17GUIZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410219787.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2026-11-17
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

The existing CLAM steel has insufficient high-temperature mechanical properties, especially poor creep properties, and traditional treatment methods are difficult to effectively improve its upper limit of service temperature.

Method used

A deformation heat treatment method for controlling TaC in CLAM steel was adopted, including austenitization, isothermal treatment, hot deformation and tempering. By controlling the amount and distribution of TaC precipitation, its stability at high temperature was improved.

Benefits of technology

It significantly improves the high-temperature mechanical properties of CLAM steel, especially its creep properties, meeting the performance requirements of fusion reactor blanket structure materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064690B_ABST
    Figure CN118064690B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of nuclear material hot working and provides a method for controlling the deformation heat treatment of TaC in CLAM steel: CLAM steel is subjected to austenitization treatment at 980℃~1150℃ for 5~30 minutes, followed by isothermal treatment at 875℃~890℃ for 30~60 minutes, then air-cooled to 830℃~870℃ for 30%~60% hot deformation, followed by water quenching to room temperature, and finally tempering at 760℃ for 90~120 minutes, after which it is air-cooled to room temperature. The deformation heat treatment process proposed in this invention can significantly increase the bulk density and volume fraction of TaC while causing a large amount of TaC to precipitate at the lath interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nuclear material heat treatment, specifically relating to a method for controlling the deformation heat treatment of TaC in CLAM steel. Background Technology

[0002] Thermonuclear fusion energy is considered humanity's ultimate energy source due to its abundant raw materials, safe operation, and large energy release. CLAM steel (China Low Activation Mantensitic steel) is a cladding structure material for thermonuclear fusion reactors, independently developed in my country. Traditional normalizing and tempering treatments limit the upper limit of CLAM steel's operating temperature to only 550℃. To improve the thermoelectric conversion efficiency of fusion reactors, it is necessary to increase the upper limit of CLAM steel's operating temperature, which means improving its high-temperature mechanical properties, especially creep resistance.

[0003] The key to increasing the service temperature of CLAM steel lies in suppressing dislocation recovery and microstructure coarsening. From the perspective of the strengthening mechanism of CLAM steel, this means maximizing the composite strengthening mechanism formed by dislocation strengthening, precipitation strengthening, and interface strengthening. Specifically, this is achieved by precipitating relative dislocations and pinning interfaces to delay microstructure degradation. CLAM steel mainly contains two precipitated phases: Cr23C6 and TaC. Cr23C6 is abundant at various interfaces and always precipitates before TaC during tempering. The first-precipitated Cr23C6 preferentially occupies high-energy sites such as grain boundaries, making it prone to coarsening during high-temperature service and degrading the material's high-temperature performance. TaC, on the other hand, has strong thermal stability and a low coarsening rate at high temperatures. It is mainly distributed at martensitic lath boundaries and within laths, which is very beneficial for improving the high-temperature creep resistance of CLAM steel. By employing effective hot working processes to control TaC and increase its precipitation, the high-temperature mechanical properties of CLAM steel can be significantly improved, thereby achieving the goal of increasing the upper limit of its service temperature. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method for controlling the deformation heat treatment of TaC in CLAM steel, thereby solving the problems in the prior art. The technical solution adopted by this invention is as follows:

[0005] A method for controlling the deformation heat treatment of TaC in CLAM steel, comprising the following steps:

[0006] Step 1, austenitizing treatment: The CLAM steel is austenitized and then air-cooled to the isothermal treatment temperature;

[0007] Step 2, isothermal treatment: Hold the temperature at the isothermal treatment temperature for a certain period of time, and then air cool to the heat distortion temperature;

[0008] Step 3, hot deformation treatment: hot deformation with a certain engineering strain is performed at the hot deformation temperature, and the steel is immediately water-cooled to room temperature after hot deformation to obtain quenched CLAM steel;

[0009] Step 4, tempering treatment: The quenched CLAM steel is tempered and then air-cooled to room temperature to obtain tempered CLAM steel.

[0010] Furthermore, in step 1, the austenitizing temperature is 980℃~1150℃, and the holding time is 5~30 minutes.

[0011] Furthermore, in step 2, the isothermal treatment temperature is 875℃~890℃, and the isothermal duration is 30~60 minutes.

[0012] Furthermore, in step 3, the heat distortion temperature is 830℃~870℃, and the engineering strain is 30%~60%.

[0013] Furthermore, in step 4, the tempering temperature is 760°C and the tempering time is 90–120 minutes.

[0014] A high TaC content CLAM steel, obtained by the aforementioned deformation heat treatment method, meets the performance requirements of fusion reactor blanket structure materials.

[0015] The present invention has the following beneficial effects:

[0016] (1) This invention achieves the regulation of TaC in CLAM steel through special deformation heat treatment, thereby improving its high-temperature mechanical properties;

[0017] (2) The process of the present invention is simple and easy to operate, and is suitable for large-scale production. Attached Figure Description

[0018] Figure 1 Comparison of TaC bulk density between Example 1 and Comparative Example 1;

[0019] Figure 2 This is a comparison of the TaC volume fraction between Example 1 and Comparative Example 1;

[0020] Figure 3 This illustrates the precipitation at the slat interface in Example 1.

[0021] Figure 4 This is a comparison of the precipitation at the slat interface in Example 1. Detailed Implementation

[0022] The following will be based on embodiments of the present invention. Figures 1-4The technical solutions in the embodiments of the present invention will be clearly and completely described. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0023] A method for controlling the deformation heat treatment of TaC in CLAM steel, comprising the following steps:

[0024] Step 1, austenitizing treatment: The CLAM steel is austenitized and then air-cooled to the isothermal treatment temperature;

[0025] Step 2, isothermal treatment: Hold the temperature at the isothermal treatment temperature for a certain period of time, and then air cool to the heat distortion temperature;

[0026] Step 3, hot deformation treatment: hot deformation with a certain engineering strain is performed at the hot deformation temperature, and the steel is immediately water-cooled to room temperature after hot deformation to obtain quenched CLAM steel;

[0027] Step 4, tempering treatment: The quenched CLAM steel is tempered and then air-cooled to room temperature to obtain tempered CLAM steel.

[0028] Furthermore, in step 1, the austenitizing temperature is 980℃~1150℃, and the holding time is 5~30 minutes.

[0029] Furthermore, in step 2, the isothermal treatment temperature is 875℃~890℃, and the isothermal duration is 30~60 minutes.

[0030] Furthermore, in step 3, the heat distortion temperature is 830℃~870℃, and the engineering strain is 30%~60%.

[0031] Furthermore, in step 4, the tempering temperature is 760°C and the tempering time is 90–120 minutes.

[0032] A high TaC content CLAM steel obtained by the aforementioned deformation heat treatment method can meet the performance requirements of fusion reactor blanket structure materials.

[0033] The advantages of the present invention are illustrated below with an example and comparative examples:

[0034] Referring to the table below, the CLAM steel alloy composition (wt.%) used in Example 1 and Comparative Example 1 of this invention is shown.

[0035]

[0036] Example 1:

[0037] Step 1, austenitizing treatment: Heat the CLAM steel to 1150℃ at a heating rate of 5℃ / s and hold at this temperature for 5 minutes; (The purpose of rapid heating and short holding time is twofold: firstly, to allow the second phase in the material to fully dissolve in the matrix, and secondly, to prevent grain growth.)

[0038] Step 2, isothermal treatment: Based on Step 1, air cool to 880℃ and hold for 30 minutes; (This step is to allow only TaC to precipitate, while preventing C23C6 from precipitating. On the one hand, this can increase the amount of TaC precipitation, and on the other hand, the precipitation of TaC can consume some of the C in the steel, reducing the precipitation of coarse C23C6 phases during subsequent tempering, which is beneficial for controlling nano-precipitates)

[0039] Step 3, Hot Deformation Treatment: Based on Step 2, air-cool to 850℃ and perform hot deformation with an engineering strain of 60%. After deformation, immediately water-cool to room temperature to obtain quenched CLAM steel; (The purpose of this step is to increase the interface by forming a large number of dislocations and refining the substructures such as martensite laths in the steel through deformation. The increase in dislocation density and interface is beneficial to increase the nucleation sites of precipitates during subsequent tempering, improve the number density of precipitates, refine the precipitates, achieve dispersion strengthening, and improve the room temperature and high temperature mechanical properties of the steel.)

[0040] Step 4, Tempering: The quenched CLAM steel is tempered at 760℃ for 90 minutes, and then air-cooled to room temperature to obtain tempered CLAM steel. (The purpose of this step is to obtain a large amount of dispersed Cr23C6, which improves the mechanical properties of CLAM steel).

[0041] Comparative Example 1 (without isothermal treatment):

[0042] Step 1, austenitizing treatment: Heat CLAM steel to 1150℃ at a heating rate of 5℃ / s, and hold at this temperature for 5 minutes;

[0043] Step 2, hot deformation treatment: Based on Step 1, air cool to 850℃ and perform hot deformation with an engineering strain of 60%. After deformation, immediately water cool to room temperature to obtain quenched CLAM steel.

[0044] Step 3, tempering treatment: The quenched CLAM steel is tempered at 760℃ for 90min, and then air-cooled to room temperature to obtain tempered CLAM steel.

[0045] Compared to Comparative Example 1, the TaC bulk density of the CLAM steel treated with Example 1 of the present invention increased by 88%, see Figure 1 The TaC volume fraction increased by 34.1%, see [link to article]. Figure 2Example 1 showed that a large amount of TaC precipitated at the lath interface, see... Figure 3 The precipitated phase on the lath interface of Comparative Example 1 was mainly Cr23C6, see [reference needed]. Figure 4 Therefore, the deformation heat treatment process proposed in this invention can significantly increase the bulk density and volume fraction of TaC while causing a large amount of TaC to precipitate at the lath interface.

[0046] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Any modifications, alterations, substitutions, or variations made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention shall fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for controlling the deformation heat treatment of TaC in CLAM steel, characterized in that, Includes the following steps: Step 1, austenitizing treatment: The CLAM steel is austenitized and then air-cooled to the isothermal treatment temperature; Step 2, isothermal treatment: Hold the temperature at the isothermal treatment temperature for a certain period of time, and then air cool to the heat distortion temperature; Step 3, hot deformation treatment: hot deformation with a certain engineering strain is performed at the hot deformation temperature, and the steel is immediately water-cooled to room temperature after hot deformation to obtain quenched CLAM steel; Step 4, tempering treatment: The quenched CLAM steel is tempered and then air-cooled to room temperature to obtain tempered CLAM steel; In step 2, the isothermal treatment temperature is 875℃~890℃, and the isothermal duration is 30~60 minutes; In step 3, the heat distortion temperature is 830℃~870℃, and the engineering strain is 30%~60%. In step 4, the tempering temperature is 760℃ and the tempering time is 90~120 minutes. Step 1, austenitizing treatment: Heat CLAM steel to 1150℃ at a heating rate of 5℃ / s, and hold at this temperature for 5 minutes.

2. A high TaC content CLAM steel, obtained by the deformation heat treatment method as described in claim 1, which meets the performance requirements of fusion reactor blanket structure materials.

Citation Information

Patent Citations

  • CLAM steel strengthening method

    CN109457095A

  • Si-containing low activation martensitic steel and heat treatment method thereof

    CN109609849A