An Al-Si-C alloy for inhibiting Si particle coarsening, its preparation method and application

By adding petroleum coke to Al-Si alloys and performing high-speed ball milling and pressing, the problem of Si particle coarsening was solved, and the mechanical properties and thermal stability of Al-Si alloys were improved, making them suitable for aerospace, automotive parts and other fields.

CN118064768BActive Publication Date: 2026-11-17NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410209649.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2026-11-17
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

In the process of preparing Al-Si alloy powder by mechanical alloying and hot solidification forming, Si particles are prone to coarsening, which affects the strength and plasticity of the material. In addition, the material is highly sensitive to quenching and its performance is reduced during aging heat treatment.

Method used

Petroleum coke was added to Al-Si alloy, and after uniform mixing by high-speed ball milling, it was pressed and further processed to prepare Al-Si-C alloy. The petroleum coke was dispersed in the aluminum matrix, which hindered the diffusion of Si element and suppressed the coarsening of Si particles.

Benefits of technology

It effectively inhibits Si particle coarsening, improves the mechanical properties of Al-Si alloys, enhances material strength and plasticity, reduces Si particle agglomeration, and strengthens the thermal stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064768B_ABST
    Figure CN118064768B_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal material preparation technology, specifically to an Al-Si-C alloy for suppressing Si particle coarsening, its preparation method, and its application. The Al-Si-C alloy comprises 0.1%–5% carbon material by mass and 95%–99.9% Al-Si matrix material, with the carbon material being petroleum coke. The mass percentage of Si in the Al-Si matrix material is ≤12%. Adding petroleum coke during the mechanical alloying process accelerates the welding-crushing process of the Al-Si alloy powder, simultaneously obtaining a composite powder with uniformly dispersed ultrafine Si particles. By adding petroleum coke, elements such as H, O, N, and S are simultaneously introduced into the aluminum matrix, achieving dispersed distribution of C particles within the aluminum matrix. H, O, N, and S elements achieve supersaturated solid solution and uniform distribution within the aluminum matrix. The multi-element coupled lattice distortion synergistically induces a pinning effect in C particles, hindering the diffusion behavior of Si elements in the aluminum matrix, improving the thermal stability of Si particles, and avoiding coarsening and agglomeration of Si particles during powder solidification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal material preparation technology, specifically to an Al-Si-C alloy for inhibiting Si particle coarsening, its preparation method, and its application. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] Aluminum-based composites are the most studied and important type of metal matrix composites. Currently, the main aluminum-based composite systems include SiC / Al, Si / Al, B4C / Al, and Al2O3 / Al. ​​Among them, Al-Si series cast aluminum alloys have advantages such as high specific strength and specific stiffness, good casting performance, low coefficient of thermal expansion and hot cracking tendency, and excellent corrosion resistance, and are widely used in automotive, communications, electronics, and machinery industries.

[0004] The main preparation methods for Al-Si alloys include melting and casting and powder metallurgy. Melting and casting involves liquefying aluminum alloy at high temperatures, then adding Si, resulting in a dispersed Si distribution within the solid matrix. Powder metallurgy involves mixing Si with aluminum alloy powder and hot-pressing or extrusion sintering above the solidus temperature. Research has found that simply optimizing the melting and casting process—including improving purity, adjusting composition, and modifying heat treatment specifications—has increasingly limited effectiveness in improving the performance of aluminum-based materials. However, powder metallurgy can avoid material segregation, refine the microstructure, and improve the morphology and distribution of reinforcing phases, offering significant advantages in preparing high-performance aluminum alloys.

[0005] When preparing Al-Si alloys using mechanical alloying, the diffusion rate of Si in Al increases significantly with increasing temperature. During the powder thermosetting process, the diffusion behavior of Si in Al will cause coarsening of Si particles. Coarse Si particles are prone to cracking during plastic deformation, affecting the strength and plasticity of the material. Furthermore, this high diffusion behavior of Si makes Al-Si alloys highly sensitive to quenching, reduces the peak performance of the material during aging heat treatment, and has poor hardenability, which is not conducive to the preparation of large-sized workpieces with thick cross-sectional areas. Summary of the Invention

[0006] To overcome the above problems, this invention provides an Al-Si-C alloy that suppresses Si particle coarsening, its preparation method, and its application. By adding petroleum coke to the Al-Si alloy, this invention can effectively solve the problem of Si particle coarsening during the hot solidification forming process of mechanical alloying to prepare Al-Si alloy powder.

[0007] To achieve the above technical objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an Al-Si-C alloy for suppressing Si particle coarsening, comprising 0.1% to 5% carbon material by mass fraction and 95% to 99.9% Al-Si matrix material; The carbon material is petroleum coke; the mass percentage of Si in the Al-Si matrix material is ≤12%.

[0008] A second aspect of the present invention provides a method for preparing the above-mentioned Al-Si-C alloy, comprising: (1) The carbon material and Al-Si matrix material are mixed evenly using a high-speed ball milling process according to the formula to obtain Al-Si-C alloy powder; (2) Press the Al-Si-C alloy powder obtained in step (1) and then perform subsequent processing to obtain the Al-Si-C alloy.

[0009] In one or more embodiments, the particle size of the carbon material is 100~300 nm.

[0010] In one or more embodiments, the Al-Si matrix material is an atomized powder with a particle size of 1~200 μm.

[0011] In one or more embodiments, in the high-speed ball milling process, the ball mill rotation speed is 300~500 rpm and the ball milling time is 0.5~20 h.

[0012] In one or more embodiments, in step (2), the Al-Si-C alloy powder obtained in step (1) is pressed at a pressure higher than 100 MPa.

[0013] In one or more embodiments, in step (2), the subsequent processing technology includes one or more of the following processing technologies: sintering, extrusion, forging and rolling.

[0014] A third aspect of the present invention provides the application of the above-mentioned Al-Si-C alloy in aerospace components, high-speed rail components, and automotive components.

[0015] The beneficial effects of this invention are as follows: (1) Adding petroleum coke during the mechanical alloying process of Al-Si alloy can accelerate the welding-crushing process of Al-Si alloy powder and obtain composite powder with uniformly dispersed ultrafine Si particles. By adding petroleum coke, elements such as H, O, N and S are introduced into the aluminum matrix at the same time, realizing the dispersed distribution of C particles in the aluminum matrix, and achieving supersaturated solid solution and uniform distribution of H, O, N and S elements in the aluminum matrix. The multi-element coupled lattice distortion synergistically creates the pinning effect of C particles, which hinders the diffusion behavior of Si elements in the aluminum matrix, improves the thermal stability of Si particles, and avoids the coarsening and agglomeration of Si particles during the powder solidification process; thus significantly improving the mechanical properties of Al-Si alloy.

[0016] (2) The petroleum coke material used in this invention is a by-product of the petroleum industry, with large output and low cost. At the same time, petroleum coke contains a lot of metallic impurities, which, as an Al-Si alloy reinforcement, is conducive to achieving metallurgical bonding between the C phase and the aluminum matrix, thereby improving the strength and plasticity of the Al-Si alloy. Therefore, petroleum coke has broad application prospects as a reinforcement material for Al-Si alloys. Attached Figure Description

[0017] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0018] Figure 1 Image a is a scanning electron microscope (SEM) image of Al-12Si alloy gas-atomized powder; image b is a scanning electron microscope (SEM) image of the Al-Si-C alloy product synthesized in Example 1. Figure 2 The image shows a scanning electron microscope (SEM) image of the Al-Si alloy product synthesized in Comparative Example 1. Detailed Implementation

[0019] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0020] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, the singular form is intended to include the plural form unless otherwise explicitly indicated by the context. Furthermore, it should be understood that when the terms “comprising” and / or “including” are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0021] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.

[0022] Example 1 An Al-Si-C alloy comprising 2% petroleum coke by mass and 98% Al-12Si alloy gas atomization powder.

[0023] Preparation method: (1) Petroleum coke was mechanically crushed to obtain a particle size of 300 nm. The petroleum coke powder and Al-12Si alloy gas atomized powder with an average particle size of 1 μm were mixed evenly using a variable speed ball milling process with a high speed ball mill to obtain Al-Si-C alloy powder. The high speed ball milling process was carried out at a rotation speed of 400 rpm for 12 h.

[0024] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 ℃ and an extrusion ratio of 10 to obtain Al-Si-C alloy products.

[0025] Scanning electron microscope (SEM) images of the Al-12Si alloy atomized powder and the synthesized Al-Si-C alloy product in this embodiment are as follows: Figure 1 The image shown is a scanning electron microscope image of Al-12Si alloy gas-atomized powder. Figure 1 No Si phase was found in (a) of the sample. This is mainly due to the rapid cooling rate during gas atomization, resulting in supersaturated solid solution of Si in the aluminum matrix. Scanning electron microscope images of the synthesized Al-Si-C alloy products ( Figure 1 As can be seen in b), a large number of Si phase particles with a size of about 150 nm are uniformly dispersed in the aluminum matrix. This is due to the precipitation of Si phase during the hot extrusion process.

[0026] The yield strength, tensile strength, and elongation of the Al-Si-C alloy product prepared in this embodiment are 375 MPa, 452 MPa, and 7.2%, respectively.

[0027] Comparative Example 1: Compared to Example 1, no petroleum coke was added. Al-12Si alloy gas-atomized powder with an average particle size of 1 μm was uniformly mixed using a variable-speed ball milling process with high speed to obtain Al-Si alloy powder. The high-speed ball milling was performed at a rotation speed of 400 rpm for 12 h.

[0028] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 °C and an extrusion ratio of 10 to obtain Al-Si alloy products.

[0029] Figure 2 Scanning electron microscope (SEM) images of the Al-Si alloy products prepared in this comparative example are shown below. Figure 2 As can be seen, Si particles are uniformly distributed in the aluminum matrix, with an average particle size of about 1.5 μm. During the hot extrusion process, supersaturated solid solution Si elements precipitate to form Si particles, which then grow. Compared with Example 1, it can be seen that the introduction of petroleum coke has a very obvious effect on inhibiting the growth of Si particles.

[0030] The yield strength, tensile strength, and elongation of the Al-Si alloy product obtained in this comparative example were 284 MPa, 328 MPa, and 5.8%, respectively.

[0031] Comparative Example 2: Compared to Example 1, petroleum coke was replaced with graphene. An Al-Si-C alloy comprising 2% graphene by mass and 98% Al-12Si alloy gas-atomized powder.

[0032] Preparation method: (1) Graphene with a sheet diameter of 20 μm and a thickness of 5 nm and Al-12Si alloy gas atomized powder with an average particle size of 1 μm were mixed uniformly using a variable speed ball milling process with high speed ball milling to obtain Al-Si-C alloy powder. The high speed ball milling was carried out at a rotation speed of 400 rpm for 12 h.

[0033] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 ℃ and an extrusion ratio of 10 to obtain Al-Si-C alloy products.

[0034] The yield strength, tensile strength, and elongation of the Al-Si-C alloy product prepared in this comparative example are 308 MPa, 352 MPa, and 5.3%, respectively.

[0035] Example 2 The alloy products obtained in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to aging treatment at a temperature of 160 °C for 6 h. After aging treatment, they were allowed to cool naturally. The mechanical properties of the alloy products after aging treatment were then tested.

[0036] In Example 1, after aging treatment, the yield strength, tensile strength, and elongation of the alloy product were 468 MPa, 541 MPa, and 5.7%, respectively.

[0037] After aging treatment, the alloy product obtained in Comparative Example 1 had a yield strength, tensile strength, and elongation of 324 MPa, 357 MPa, and 4.3%, respectively.

[0038] After aging treatment, the alloy product obtained in Comparative Example 2 had a yield strength, tensile strength, and elongation of 372 MPa, 403 MPa, and 3.8%, respectively.

[0039] Example 3: Compared with Example 1, the content of petroleum coke was changed. An Al-Si-C alloy comprising 5% petroleum coke by mass and 95% Al-12Si alloy gas atomization powder.

[0040] Preparation method: (1) Petroleum coke was mechanically crushed to obtain a particle size of 300 nm. The petroleum coke powder and Al-12Si alloy gas atomized powder with an average particle size of 1 μm were mixed evenly using a variable speed ball milling process with a high speed ball mill to obtain Al-Si-C alloy powder. The high speed ball milling process was carried out at a rotation speed of 400 rpm for 12 h.

[0041] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 ℃ and an extrusion ratio of 10 to obtain Al-Si-C alloy products.

[0042] In this embodiment, the yield strength, tensile strength, and elongation of the Al-Si-C alloy product obtained are 401 MPa, 493 MPa, and 5.8%, respectively.

[0043] Example 4: Compared with Example 1, the content of petroleum coke was changed. An Al-Si-C alloy comprising 0.1% petroleum coke by mass and 99.9% Al-12Si alloy gas atomization powder.

[0044] Preparation method: (1) Petroleum coke was mechanically crushed to obtain a particle size of 300 nm. The petroleum coke powder and Al-12Si alloy gas atomized powder with an average particle size of 1 μm were mixed evenly using a variable speed ball milling process with a high speed ball mill to obtain Al-Si-C alloy powder. The high speed ball milling process was carried out at a rotation speed of 400 rpm for 12 h.

[0045] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 ℃ and an extrusion ratio of 10 to obtain Al-Si-C alloy products.

[0046] In this embodiment, the yield strength, tensile strength, and elongation of the Al-Si-C alloy product obtained are 315 MPa, 372 MPa, and 6.4%, respectively.

[0047] Example 5: Compared with Example 1, the subsequent processing technology was changed. An Al-Si-C alloy comprising 2% petroleum coke by mass and 98% Al-12Si alloy gas atomization powder.

[0048] Preparation method: (1) Petroleum coke was mechanically crushed to obtain a particle size of 300 nm. The petroleum coke powder and Al-12Si alloy gas atomized powder with an average particle size of 1 μm were mixed evenly using a variable speed ball milling process with a high speed ball mill to obtain Al-Si-C alloy powder. The high speed ball milling process was carried out at a rotation speed of 400 rpm for 12 h.

[0049] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then sintered at a temperature of 450 °C for 1 h to obtain Al-Si-C alloy products.

[0050] In this embodiment, the compressive yield strength and compressive strength of the Al-Si-C alloy product were 312 MPa and 624 MPa, respectively, and 50% of it did not break under compressive strain.

[0051] Example 6: Compared with Example 1, the particle size of the crushed petroleum coke and the particle size of the Al-12Si alloy gas atomization powder were changed. An Al-Si-C alloy comprising 2% petroleum coke by mass and 98% Al-12Si alloy gas atomization powder.

[0052] Preparation method: (1) Petroleum coke was mechanically crushed to obtain a particle size of 100 nm. The petroleum coke powder and Al-12Si alloy gas atomized powder with an average particle size of 200 μm were mixed evenly using a variable-speed ball milling process with a high speed to obtain Al-Si-C alloy powder. The high-speed ball milling was performed with a rotation speed of 400 rpm and a milling time of 12 h.

[0053] (2) The Al-Si-C alloy powder obtained in step (1) is pressed at a pressure of 1300 MPa and then extruded at a temperature of 400 ℃ and an extrusion ratio of 10 to obtain Al-Si-C alloy products.

[0054] In this embodiment, the yield strength, tensile strength, and elongation of the Al-Si-C alloy product obtained are 367 MPa, 443 MPa, and 8.0%, respectively.

[0055] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An Al-Si-C alloy for inhibiting Si particle coarsening, characterized in that, It includes carbon materials with a mass fraction of 0.1% to 5% and Al-Si matrix materials with a mass fraction of 95% to 99.9%. The carbon material is petroleum coke; the mass percentage of Si in the Al-Si matrix material is ≤12%. The method for preparing the Al-Si-C alloy includes: (1) The carbon material and Al-Si matrix material are mixed evenly using a high-speed ball milling process according to the formula to obtain Al-Si-C alloy powder; (2) Press the Al-Si-C alloy powder obtained in step (1) and then perform subsequent processing to obtain the Al-Si-C alloy. In the Al-Si-C alloy, C particles are dispersedly distributed in the aluminum matrix.

2. The method for preparing the Al-Si-C alloy according to claim 1, characterized in that, include: (1) The carbon material and Al-Si matrix material are mixed evenly using a high-speed ball milling process according to the formula to obtain Al-Si-C alloy powder; (2) Press the Al-Si-C alloy powder obtained in step (1) and then perform subsequent processing to obtain the Al-Si-C alloy.

3. The preparation method according to claim 2, characterized in that, The particle size of the carbon material is 100~300 nm.

4. The preparation method according to claim 2, characterized in that, The Al-Si matrix material is an atomized powder with a particle size of 1~200 μm.

5. The preparation method according to claim 2, characterized in that, In the high-speed ball milling process, the ball mill rotation speed is 300~500 rpm, and the ball milling time is 0.5~20 h.

6. The preparation method according to claim 2, characterized in that, In step (2), the Al-Si-C alloy powder obtained in step (1) is pressed at a pressure higher than 100 MPa.

7. The preparation method according to claim 2, characterized in that, In step (2), the subsequent processing technology includes one or more of the following: sintering, extrusion, forging and rolling processes.

8. The application of the Al-Si-C alloy according to claim 1 in aerospace components, high-speed rail components and automotive components.

Citation Information

Patent Citations

  • Improved thermal properties of carbon-aluminum composites

    CN102301039A