Stabilizer for cyanide-containing gold-silver electroplating solution, electroplating solution and electroplating method

By using hydantoin as a stabilizer and leveling agent in the cyano-containing silver plating solution, combining current density adjustment and conductive salt, the problems of plating solution stability and silver ion photodecomposition are solved, and high stability and It satisfies various performances and is suitable for semiconductor chip packaging.

CN118064943BActive Publication Date: 2024-12-06SHENZHEN UNITED BLUEOCEAN APPLIED MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410077009.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2024-01-10
Filing Date
2024-01-19
Publication Date
2024-12-06
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

The existing cyano-containing silver plating solution has poor stability in semiconductor chip packaging, free cyanide ions lead to photoresist swelling and silver ions photodecomposition, which is difficult to meet the needs of hardness, roughness and anti-sulfurization oxidation.

Method used

Use hydantoin or its derivatives as stabilizers, as complexing agents and leveling agents for silver ions to avoid photodecomposition of silver ions, and obtain gold and silver with different gold content by adjusting the pH value and current density of the electroplating solution. The alloy coating combines pyrophosphate as the conductive salt to form a high-stability plating solution.

Benefits of technology

A high-stability electroplating solution without the need for additional free cyanide ions is achieved, which avoids photodecomposition of silver ions, meets the semiconductor chip's demand for hardness, roughness and anti-sulfurization oxidation, and improves the plating performance through annealing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064943B_ABST
    Figure CN118064943B_ABST
Patent Text Reader

Abstract

The invention discloses a stabilizer, a plating solution and an electroplating method for a cyanide-containing gold-silver electroplating solution, and belongs to the field of electroplating technology. The stabilizer is hydantoin or a derivative thereof, and the molar ratio of the stabilizer to the silver ions in the cyanide-containing gold-silver electroplating solution is 2 or more. The gold-silver electroplating solution comprises a water-soluble cyanide-containing gold salt, a water-soluble cyanide-containing silver salt, a conductive salt, the stabilizer and water; the gold ion concentration is 1-20 g / L, the silver ion concentration is 0.3-10 g / L, and the conductive salt concentration is 10-120 g / L. The stabilizer of the invention has excellent protection ability for the silver ions in the cyanide-containing gold-silver electroplating solution, and can also act as a leveling agent; the electroplating solution has extremely high stability, does not need to add free cyanide ions and leveling agents, and is relatively friendly to the process involving photoresist in semiconductor chip manufacturing; without changing the electroplating equipment and the electroplating solution, only the current density needs to be changed to obtain a gold-silver alloy coating with different gold contents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating, and relates to a stabilizer for a cyanide-containing gold-silver electroplating solution, an electroplating solution and an electroplating method. The gold-silver electroplating solution has high stability and does not contain free cyanide ions, and is suitable for semiconductor chips. Background Art

[0002] When semiconductor chips are packaged, pure gold is usually used to prepare the packaging structure in order to ensure chip performance based on the excellent properties of gold. If silver can partially replace gold, the cost of the packaging structure can be greatly reduced; and gold-silver alloy has lower resistance and higher thermal conductivity than pure gold, which helps to improve the heat dissipation performance of the chip and increase the interconnection density of electrical appliances.

[0003] The use of electroplating technology to prepare gold-silver alloy packaging structures instead of pure gold packaging structures has some technical requirements for gold-silver electroplating solutions that are the same as other application scenarios, such as high stability; and some requirements that are different from other application scenarios, such as: (1) it must not cause the photoresist on the chip to be packaged to swell, and (2) it must be convenient to manufacture gold-silver coatings with different gold contents to form a composite structure to simultaneously meet the packaging structure's multiple requirements for hardness, roughness, and resistance to sulfurization and oxidation.

[0004] Gold-silver alloy electroplating solutions are divided into two categories: those containing cyanide and those not containing cyanide. Among them, due to the high complex constants of gold ions, silver ions and cyanide ions, they are more stable than those not containing cyanide. However, silver ions are photosensitive substances. In addition to the cyanide part of potassium silver cyanide, free cyanide ions are usually introduced into the plating solution to ensure that the silver ions will not decompose when exposed to light. In addition to the great safety hazards, free cyanide ions will also swell the photoresist, resulting in a decrease in the manufacturing accuracy of the circuit. Therefore, it is difficult for the industry to develop stabilizers and corresponding electroplating solutions containing cyanide gold-silver electroplating solutions that do not contain free cyanide ions and ensure high stability of the plating solution.

[0005] CN104099653B discloses a technical solution for preparing a gold-silver alloy using potassium cyanide gold and potassium silver cyanide electroplating solutions, wherein the pH of the plating solution is 6.5-7.0, and the plating solution contains 2-5 mL / L of oxalate as a leveling agent (see paragraphs 160-165 of its specification). Because the plating solution does not contain a protective agent for silver ions, such as free cyanide ions; and in addition, within the pH range, the cyanide ions provided by the main salt have poor coordination ability with silver ions, so the stability of the electroplating solution is poor.

[0006] GB2046794A and CH629260A5 also disclose technical solutions for preparing gold-silver alloys using potassium cyanide gold and potassium cyanide silver electroplating solutions. The plating solution does not contain free cyanide ions, but uses polymer additives such as polyethyleneimine or polyethylene oxide as brighteners. First, due to the lack of a protective agent for silver ions, the stability of these plating solutions is poor; second, polyethyleneimine or polyethylene oxide is easily co-deposited in the coating, resulting in excessive internal stress in the coating and formation of holes in the coating after annealing, which reduces the corrosion resistance of the coating. Summary of the invention

[0007] The purpose of the present invention is to provide a stabilizer for a cyanide-containing gold-silver electroplating solution, as well as a corresponding electroplating solution and an electroplating method. The stabilizer has excellent protection capability for silver ions in the cyanide-containing gold-silver electroplating solution, thereby preventing the silver ions from being photodecomposed, and can also function as a leveler, so that the gold-silver electroplating solution does not need to be additionally added with a leveler; the electroplating solution has extremely high stability, and does not need to be additionally added with free cyanide ions, so that the process involving photoresist in semiconductor chip manufacturing is relatively friendly; the electroplating method can conveniently obtain gold-silver alloy coatings with different gold contents, thereby obtaining a corresponding composite structure, so as to simultaneously meet the multi-faceted requirements of the semiconductor chip packaging structure on hardness, roughness and resistance to sulfidation and oxidation.

[0008] One aspect of the present invention is to provide a stabilizer for a cyanide-containing gold-silver electroplating solution. The stabilizer is hydantoin or a derivative thereof, and the molar ratio of the stabilizer to the silver ions in the cyanide-containing gold-silver electroplating solution is greater than 2, preferably 2-20.

[0009] The stabilizer hydantoin or its derivative provided by the present invention, on the one hand, acts as a complexing agent for silver ions, prevents the photoreduction of silver ions, and improves the stability of the electroplating solution. The molar ratio of hydantoin or its derivative to silver ions is above 2, preferably 2-20, to ensure the coordination and complexation with silver ions. The molar ratio of hydantoin or its derivative to silver ions is higher than 20, which may cause the viscosity of the plating solution to be too high, thereby reducing the uniformity of the electroplating thickness. On the other hand, in addition to the complexation with silver ions, hydantoin or its derivative and silver ions achieve synergistic effects and play the role of a crystallization regulator. Both silver plating and gold plating alone require the addition of a crystallization regulator in the electroplating solution, while the technical solution of the present invention does not require the addition of a crystallization regulator, and a very smooth coating can also be obtained.

[0010] Furthermore, the hydantoin derivative is 5,5-dimethylhydantoin (CAS number: 77-71-4), 1,3-dihydroxymethyl-5,5-dimethylhydantoin (CAS number: 6440-58-0) or 1-aminohydantoin (CAS number: 6301-02-6), preferably 5,5-dimethylhydantoin.

[0011] Another aspect of the present invention is to provide a gold-silver electroplating solution, which comprises a water-soluble cyanide-containing gold salt, a water-soluble cyanide-containing silver salt, a conductive salt, the above-mentioned stabilizer and water; the gold ion concentration is 1-20 g / L, the silver ion concentration is 0.3-10 g / L, and the conductive salt concentration is 10-120 g / L.

[0012] Furthermore, the pH value of the gold-silver electroplating solution is 8-10. When the pH value is lower than 8, the complexing ability of the stabilizer and silver ions decreases, resulting in poor stability of the plating solution; when the pH value is higher than 10, it will have an adverse effect on the photoresist.

[0013] Furthermore, the water-soluble cyanide-containing gold salt is preferably potassium aurous cyanide (molecular formula KAu(CN)2), and the gold ion concentration is 1-20g / L. When it is less than 1g / L, the coating is easily scorched during electroplating; when it exceeds 20g / L, the cost increases due to the effect of carryover. The water-soluble cyanide-containing silver salt is preferably potassium silver cyanide (molecular formula KAg(CN)2), and the silver ion concentration is 0.3-10g / L. According to different scene requirements, the ratio of gold and silver in the coating can be adjusted by adjusting the concentration of silver ions in the electroplating solution.

[0014] The inventors found that when the gold ions and silver ions are within the above concentration range, the gold content of the obtained gold-silver alloy coating can be changed by simply adjusting the current density using the same electroplating solution and electroplating equipment. Specifically, the gold content in the gold-silver alloy coating obtained at a lower current density is low, and the gold content in the gold-silver alloy coating obtained at a higher current density is high. The inventors also found that when the gold content in the gold-silver alloy coating is within a moderate range (20-50wt%), the hardness and roughness can meet the requirements of semiconductor chip packaging; while resistance to sulfidation and oxidation requires a gold content of more than 60wt%. Therefore, a composite packaging structure can be designed: the gold content of the main body of the packaging structure is within a moderate range, so that the hardness and roughness meet the requirements; at the same time, a protective layer with a much smaller thickness is formed on the outer surface of the main body of the packaging structure, which does not affect the overall hardness and roughness, and meets the requirements of resistance to sulfidation and oxidation.

[0015] Furthermore, the conductive salt is preferably pyrophosphate, which can be one or more of sodium pyrophosphate, potassium pyrophosphate or ammonium pyrophosphate. Pyrophosphate can improve the conductivity of the plating solution and improve the uniformity of electroplating. Too low a concentration cannot meet the conductivity requirements of the plating solution, and too high a concentration will lead to high viscosity of the plating solution, thereby affecting the electrodeposition of gold or silver.

[0016] Another aspect of the present invention is to provide an electroplating method, using the above-mentioned gold and silver electroplating solution for electroplating, the electroplating operation temperature is 20-40°C, the electroplating current density is 0.3-1.5A / dm 2When the operating temperature is lower than 20℃, the temperature is not easy to control and the uniformity of electroplating becomes worse; when it exceeds 40℃, the roughness of the coating tends to increase, which may affect the subsequent welding performance or bonding effect. The current density of electroplating is operated at 0.3-1.5A / dm 2 Within the range, for the same composition of the electroplating solution, the gold content in the plated layer increases with increasing current density. 2 When the current density is greater than 1.5A / dm 2 There is a risk of the coating being burned.

[0017] Furthermore, when the gold content in the gold-silver plating layer is required to be below 50wt%, the current density of the electroplating is 0.3-0.6A / dm 2 When the gold content in the gold-silver plating layer is required to be above 60wt%, the current density of electroplating is 1.1-1.5A / dm 2 .

[0018] Further, the obtained gold-silver alloy electroplated layer is annealed at a temperature of 270-300° C. and an annealing time of 5-120 min. Through annealing, stress can be eliminated and the performance of the gold-silver alloy electroplated layer can be improved. The annealing temperature and annealing time can be determined by experiments within the above parameter range according to the area and thickness of the gold-silver alloy electroplated layer. The general rule is that the larger the area and the thicker the thickness, the higher the annealing temperature and the longer the annealing time required.

[0019] Another aspect of the present invention is to provide a product obtained by the above electroplating method.

[0020] The present invention has the following beneficial technical effects: the stabilizer provided by the present invention has excellent protection ability for silver ions in cyanide-containing gold-silver electroplating solution, avoids the photodecomposition of silver ions, and can also act as a leveling agent. The electroplating solution provided by the present invention has extremely high stability, does not require the additional addition of free cyanide ions, is relatively friendly to the process involving photoresist in semiconductor chip manufacturing, and does not require the additional addition of a leveling agent. The electroplating method provided by the present invention can obtain gold-silver alloy coatings with different gold contents by only changing the current density without changing the electroplating equipment and the electroplating solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the gold-silver alloy packaging structure obtained by using the electroplating solution provided by the present invention.

[0022] Figure numerals: 1-gold-silver alloy packaging structure body, 2-thin layer with high gold content, 3-chip substrate. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings of the specification. Obviously, the described implementation is only a part of the implementation of the present invention, not all of the implementations. Based on the implementation of the present invention, all other implementations obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The present invention uses the following analytical test methods to test the gold-silver electroplating solutions and gold-silver alloy coatings obtained in various embodiments and comparative examples.

[0025] (1) Stability test of the plating solution. After the plating solution is prepared, it is placed at room temperature for 24 hours. If the plating solution is clear and no metal film is formed on the surface of the plating solution, it is considered to be stable. If the plating solution is turbid or a metal film is formed on the surface of the liquid, it is considered to be unstable.

[0026] (2) Gold content test of the coating. A 300 nm TiW and an 80 nm Au seed layer were first deposited on the silicon wafer by PVD sputtering, and then a gold-silver alloy was electroplated on the test piece. The gold-silver content in the coating was tested using SEM-EDX (Zeiss, Sigma300).

[0027] (3) Roughness test of the coating. A 300 nm TiW and 80 nm Au seed layer was first deposited on the silicon wafer by PVD sputtering, and then a gold-silver alloy was electroplated on the test piece. The roughness of the coating was tested using a laser confocal microscope (KEYENCE, VK-2050).

[0028] (4) Hardness test of the coating. A 300 nm TiW and 80 nm Au seed layer was first deposited on the silicon wafer by PVD sputtering, and then a 10 μm thick gold-silver alloy was electroplated on the test piece. The hardness of the coating was tested using a hardness tester (Mitutoyo, HM-200). Example 1

[0029] First, add 600mL of deionized water to a 1L beaker, then add 60g of potassium pyrophosphate and 30g of hydantoin to fully dissolve, then add 10g of potassium cyanide gold ion content and 5g of potassium cyanide silver ion content (hydantoin to silver ion molar ratio is 6.5), adjust the pH of the plating solution to 9, and add deionized water to make the volume of the plating solution 1000mL. The electroplating temperature is set to 30℃, a 3´3cm gold-plated silicon wafer is used, and the current density is 0.3A / dm 2 , the electroplating thickness is 10 μm. The annealing temperature after electroplating is 290°C, and the annealing time is 30 minutes.

[0030] The gold content in the coating after electroplating is 26wt%, the roughness Ra is 57nm, the hardness of the coating before annealing is 102HV, the hardness of the coating after annealing is 65HV, and the plating solution is stable after being placed for 24 hours. Example 2

[0031] The difference from Example 1 is that the current density is changed to 0.4A / dm 2 , the other conditions are the same.

[0032] The gold content in the coating after electroplating is 31wt%, the roughness Ra is 63nm, the hardness of the coating before annealing is 113HV, the hardness of the coating after annealing is 62HV, and the plating solution is stable after being placed for 24 hours. Example 3

[0033] Same as Example 1 except that the current density is changed to 0.5A / dm 2 , the other conditions are the same.

[0034] The gold content in the coating after electroplating is 44wt%, the roughness Ra is 83nm, the hardness of the coating before annealing is 133HV, the hardness of the coating after annealing is 95HV, and the plating solution is stable after being placed for 24 hours. Example 4

[0035] The difference from Example 1 is that the gold ion concentration is changed to 20 g / L, the silver ion concentration is changed to 10 g / L, the potassium pyrophosphate concentration is changed to 120 g / L, the stabilizer is changed to 23.7 g / L of 5,5-dimethylhydantoin (the molar ratio of 5,5-dimethylhydantoin to silver ion is 2), the pH is changed from 9 to 8, and the temperature is changed to 20° C.; the other conditions are the same.

[0036] The gold content in the coating after electroplating is 38wt%, the roughness Ra is 82nm, the hardness of the coating before annealing is 112HV, the hardness of the coating after annealing is 85HV, and the plating solution is stable after being placed for 24 hours. Example 5

[0037] The difference from Example 4 is that the pH is changed to 10, the electroplating temperature is changed to 40°C, and the current density is changed to 0.6A / dm 2 ; The other conditions are the same.

[0038] The gold content in the coating after electroplating is 49wt%, the roughness Ra is 91nm, the hardness of the coating before annealing is 157HV, the hardness of the coating after annealing is 104HV, and the plating solution is stable after being placed for 24 hours. Example 6

[0039] The difference from Example 4 is that the pH is changed to 9, the electroplating temperature is changed to 30°C, and the current density is changed to 0.9A / dm 2 ; The other conditions are the same.

[0040] The gold content in the coating after electroplating is 57wt%, the roughness Ra is 158nm, the hardness of the coating before annealing is 177HV, the hardness of the coating after annealing is 136HV, and the plating solution is stable after being placed for 24 hours. Example 7

[0041] The difference from Example 1 is that the current density is changed to 1.0A / dm 2 , the electroplating thickness was changed to 0.5μm; the other conditions were the same.

[0042] The gold content in the plated layer after electroplating is 66wt%, the roughness Ra is 24nm, and the plating solution is stable after being left for 24 hours. Example 8

[0043] The difference from Example 1 is that the current density is changed to 1.3A / dm 2 , the electroplating thickness was changed to 0.5μm; the other conditions were the same.

[0044] The gold content in the plated layer after electroplating is 73wt%, the roughness Ra is 27nm, and the plating solution is stable after being left for 24 hours. Example 9

[0045] The difference from Example 1 is that the current density is changed to 1.6A / dm 2 , the plating thickness was changed to 0.5μm, and the other conditions were the same.

[0046] The gold content in the plated layer after electroplating is 77wt%, the roughness Ra is 34nm, and the plating solution is stable after being left for 24 hours. Example 10

[0047] The difference from Example 1 is that the gold ion concentration is changed to 1 g / L, the silver ion concentration is changed to 0.3 g / L, the potassium pyrophosphate concentration is changed to 10 g / L, the stabilizer is changed to 4.7 g / L of 5,5-dimethylhydantoin (the molar ratio of 5,5-dimethylhydantoin to silver ions is 19.8), the electroplating temperature is changed to 40° C., and the electroplating thickness is changed to 0.5 μm; the other conditions are the same.

[0048] The gold content in the plated layer after electroplating is 35wt%, the roughness Ra is 12nm, and the plating solution is stable after being left for 24 hours.

[0049] Comparative Example 1

[0050] The difference from Example 3 is that the hydantoin content is changed to 0 g / L (ie, no hydantoin is added), and the other conditions are the same.

[0051] The gold content in the coating after electroplating is 38wt%, the roughness Ra is 83nm, the hardness of the coating before annealing is 135HV, the hardness of the coating after annealing is 78HV, and a layer of silver film is found on the surface of the coating after the plating solution is left for 24 hours.

[0052] Comparative Example 2

[0053] The difference from Example 3 is that the hydantoin is changed to 5 g / L (the molar ratio of hydantoin to silver ions is changed to 1.1), and the other conditions are the same.

[0054] The gold content in the coating after electroplating is 40wt%, the roughness Ra is 79nm, the hardness of the coating before annealing is 145HV, the hardness of the coating after annealing is 85HV, and a layer of silver film is found on the surface of the coating after the coating is left in the plating solution for 24 hours.

[0055] Comparative Example 3

[0056] The difference from Example 3 is that 30 g / L of hydantoin is replaced by 5 g / L of sodium oxalate monohydrate, and the other conditions are the same.

[0057] The gold content in the coating after electroplating is 35wt%, the roughness Ra is 155nm, the hardness of the coating before annealing is 127HV, the hardness of the coating after annealing is 74HV, and a layer of silver film is found on the surface of the coating after the plating solution is left for 24 hours.

[0058] Comparative Example 4

[0059] The difference from Example 3 is that 30 g / L of hydantoin is replaced by 15 g / L of ethylenediamine, and the other conditions are the same.

[0060] The gold content in the coating after electroplating is 37wt%, the roughness Ra is 340nm, the hardness of the coating before annealing is 168HV, the hardness of the coating after annealing is 126HV, and the plating solution is stable after being placed for 24 hours.

[0061] The parameter conditions and performance comparison results of the above embodiments and comparative examples are shown in Table 1.

[0062] Table 1 Parameters and performance comparison results of various embodiments and comparative examples

[0063]

[0064] Note: “NA” in the table means “Not Applicable”.

[0065] It can be concluded from the data in Table 1 that in each embodiment, since the stabilizer of the present invention is added to the plating solution, no silver film is produced on the surface of the plating solution after the plating solution is placed for 24 hours, indicating that the stabilizer of the present invention solves the stability problem of the plating solution.

[0066] It can also be concluded from the data in Table 1 that the annealing hardness and roughness of the coating are closely related to the gold content in the coating. When the gold content in the coating is controlled below 50wt%, the roughness Ra of the coating is lower than 100nm and the annealing hardness of the coating is less than 105HV. This is of great significance for replacing pure gold with gold-silver alloy in semiconductor chip packaging structures. By comparing Examples 1-3, Examples 4-6 and Examples 7-9, it can be seen that increasing the current density can increase the gold content in the coating. Considering that gold-silver alloys, especially gold-silver alloys with lower gold content, are less resistant to oxidation or sulfidation than pure gold, this also provides a method for manufacturing gold-silver alloys with higher gold content, thereby improving the oxidation resistance or sulfidation performance of the gold-silver packaging structure. But there is a problem here that when the gold content is high, such as Example 6, the roughness and annealing hardness of the coating are large (gold is higher than 50wt%), which is not suitable for semiconductor chip packaging (generally, the roughness Ra required for packaging is less than 100nm and the annealing hardness is less than 120HV). Based on this, a two-layer packaging structure can be made using the electroplating solution of the present invention, such as Figure 1 As shown, a gold-silver alloy packaging structure body 1 with a low gold content is first prepared using a low current density, combined with a chip substrate 3 to ensure low roughness and low hardness, and the electroplating thickness is about 8-12μm; then the same electroplating solution is used on the top surface to prepare a thin layer 2 with a high gold content through a high current density to improve the anti-oxidation or anti-sulfurization performance of the gold-silver packaging structure, and the electroplating thickness is about 10-500nm. This not only ensures the requirements of low hardness and low roughness, but also ensures the reliability of subsequent welding or bonding. Examples 7-9 show that the gold-silver alloy plating layer with a high gold content has a roughness Ra of only 24-37nm when the electroplating thickness is 0.5μm.

[0067] In Comparative Example 3, sodium oxalate monohydrate was used as an additive (refer to CN104099653B). It was found that after the plating solution was placed for 24 hours, a layer of white silver film was formed on the surface of the plating solution. This was due to the photodecomposition of silver ions, indicating that sodium oxalate did not stabilize the silver ions. In Comparative Example 1, since there was no additive hydantoin derivative as a silver ion stabilizer, the plating solution was unstable after being placed for 24 hours. At the same time, it was found that the roughness of the coating was also relatively high, which again demonstrated that the synergistic effect of hydantoin and silver ions played the role of a grain regulator. In Comparative Example 2, the molar ratio of hydantoin to silver ions was less than 2. After the plating solution was placed for 24 hours, a small amount of white silver film was also found on the surface of the plating solution, indicating that a certain amount of hydantoin was needed to complex the silver ions to play the role of a stabilizer.

[0068] In addition, the synergistic use of silver ions and hydantoin or its derivatives also has the effect of a crystallization regulator. Comparing Example 3 and Comparative Example 4, at the same electroplating thickness, the roughness of the coating is 83nm when 5,5-dimethylhydantoin is used, but the roughness of the coating is 340nm when ethylenediamine is used. Although the use of ethylenediamine as an additive has a good stability of the plating solution, the roughness of the coating after electroplating is too high, and the prepared gold-silver alloy is obviously not suitable for semiconductor chip packaging.

[0069] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The protection scope of the present invention is defined by the claims and their equivalent technical solutions.

Claims

1. A gold and silver electroplating solution, characterized in that: The gold-silver electroplating solution comprises a water-soluble cyanide-containing gold salt, a water-soluble cyanide-containing silver salt, a conductive salt, a stabilizer and water, and does not need to add a crystallization regulator; the gold ion concentration is 1-20 g / L, the silver ion concentration is 0.3-10 g / L, and the conductive salt concentration is 10-120 g / L; the stabilizer is hydantoin or a derivative thereof, and the molar ratio of the stabilizer to the silver ions in the cyanide-containing gold-silver electroplating solution is greater than 2.

2. The gold-silver electroplating solution according to claim 1, characterized in that: The molar ratio of the stabilizer to the silver ions in the cyanide-containing gold-silver electroplating solution is 2-20.

3. The gold-silver electroplating solution according to claim 1, characterized in that: The hydantoin derivative is 5,5-dimethylhydantoin, 1,3-dihydroxymethyl-5,5-dimethylhydantoin or 1-aminohydantoin.

4. The gold-silver electroplating solution according to claim 3, characterized in that: The derivative of hydantoin is 5,5-dimethylhydantoin.

5. The gold-silver electroplating solution according to claim 1, characterized in that: The pH value of the electroplating solution is 8-10.

6. The gold-silver electroplating solution according to claim 1, characterized in that: The water-soluble cyanide-containing gold salt is potassium aurous cyanide, and the water-soluble cyanide-containing silver salt is potassium silver cyanide.

7. The gold-silver electroplating solution according to claim 1, characterized in that: The conductive salt is pyrophosphate.

8. The gold-silver electroplating solution according to claim 7, characterized in that: The pyrophosphate is one or more of sodium pyrophosphate, potassium pyrophosphate or ammonium pyrophosphate.

9. An electroplating method, characterized in that: The gold and silver electroplating solution according to any one of claims 1 to 8 is used for electroplating, the operating temperature of the electroplating is 20-40° C., and the current density of the electroplating is 0.3-1.5 A / dm 2 .

10. The electroplating method according to claim 9, characterized in that: When the gold content in the gold-silver plating layer is required to be below 50wt%, the current density of the electroplating is 0.3-0.6A / dm 2 When the gold content in the gold-silver plating layer is required to be above 60wt%, the current density of electroplating is 1.1-1.5A / dm 2 .

11. The electroplating method according to claim 9 or 10, characterized in that: The obtained gold-silver alloy electroplating layer is subjected to annealing treatment, the annealing temperature is 270-300° C., and the annealing time is 5-120 minutes.