A water-based polycarbodiimide crosslinking agent and its preparation method and application
The protective layer is formed through the reaction of the polycarbodiimide compound and the polyacrylic resin, which solves the problem of insufficient water resistance and chemical resistance of the water-based polycarbodiimide cross-linking agent, prolongs its use time and improves its water resistance. Coating performance.
Patent Information
- Application Number
- CN202410098526.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-24
AI Technical Summary
Existing water-based polycarbodiimide cross-linking agents have problems with insufficient water resistance and chemical resistance during use, which affects their service life and coating film performance.
A cross-linking agent having hydrophilic polyacrylic resin segments and hydrophobic polycarbodiimide compound segments is formed by reacting a polycarbodiimide compound with a polyacrylic resin containing a carboxyl group and a polyoxyalkylene segment. , forming a protective layer of polyacrylic resin to wrap the carbodiimide groups, extending its service life and improving water resistance and chemical resistance.
The cross-linking agent in water-based coatings can be used for a long time and has excellent water and chemical resistance, improving the overall performance of water-based coatings.
Smart Images

Figure BDA0004679375210000141 
Figure BDA0004679375210000151 
Figure BDA0004679375210000152
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based crosslinking agents, and in particular to a water-based polycarbodiimide crosslinking agent and a preparation method and application thereof. Background Art
[0002] In response to environmental regulations, there are more and more restrictions on volatile organic compounds in coatings. At present, water-based coatings with water as the dispersion medium have replaced traditional solvent-based resins in many fields and have been widely used.
[0003] Waterborne polycarbodiimide is an environmentally friendly crosslinking agent that can crosslink with carboxyl groups in waterborne resins (such as waterborne acrylic resins and waterborne polyurethane resins) at room temperature, which can significantly improve the chemical resistance of waterborne coatings. In addition, waterborne polycarbodiimide is insensitive to moisture and has very low toxicity, so it has been widely used.
[0004] The patent title is "Water-based resin crosslinking agent, water-based resin crosslinking agent containing liquid and water-based resin composition" (CN113490724B), which discloses a water-based carbodiimide composition, which contains a hydrophobic polycarbodiimide compound and a water-soluble organic compound, wherein the water-soluble organic compound is a nonionic surfactant. The water-based polycarbodiimide crosslinking agent obtained by this method has a long usable time, but the addition of a nonionic surfactant will also have an adverse effect on the water resistance and other properties of the crosslinking agent.
[0005] The patent name is a carbodiimide composition, a curing agent composition, a coating composition and a cured resin (CN115190901A), which discloses a carbodiimide composition, which includes a water-soluble modified polycarbodiimide and a water-insoluble polycarbodiimide, wherein the carbodiimide group in the water-soluble polycarbodiimide is modified by some small molecule compounds, and the carbodiimide group content on the surface of the dispersion particles of the carbodiimide composition is low after it is dispersed in water, so it is more difficult to react with the carboxyl-containing water-based resin, so it has a long usable time. However, this method has a high modification ratio, and a certain proportion of carbodiimide groups will be lost, which is not conducive to the improvement of crosslinking density, and will also affect water resistance and chemical resistance.
[0006] Therefore, the above methods all have some defects. The development of a water-based polycarbodiimide cross-linking agent with a long usable time and high water resistance and chemical resistance has important research significance and application value. Summary of the invention
[0007] Based on this, the purpose of the present invention is to overcome the defects or shortcomings of the prior art and provide a water-based polycarbodiimide cross-linking agent and a preparation method and application thereof. The water-based polycarbodiimide cross-linking agent has excellent water resistance and chemical resistance, and can be widely used as a cross-linking agent in water-based coatings to improve the performance of water-based coatings.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] The present invention provides a water-based polycarbodiimide crosslinking agent, which is obtained by reacting a polycarbodiimide compound (A) with a polyacrylic acid resin (B); wherein: the polyacrylic acid resin (B) contains carboxyl and polyoxyalkylene segments; the molar number of the carboxyl group of the polyacrylic acid resin (B) is 1-20% of the molar number of the carbodiimide group in the polycarbodiimide compound (A).
[0010] The water-based polycarbodiimide cross-linking agent of the present invention has a long usable time and excellent water resistance and chemical resistance, and can be widely used in water-based coatings as a cross-linking agent to improve the performance of the water-based coatings.
[0011] The inventors of the present invention have found through repeated studies that the carboxyl group in the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments will react with the carbodiimide group in the polycarbodiimide compound (A), so that the hydrophilic polyoxyalkylene segment on the polyacrylic resin (B) is introduced into the polycarbodiimide compound (A) through the reaction of the carboxyl group and the carbodiimide group, so that the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B) has good hydrophilicity and is easy to disperse in water. In the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B), the polyacrylic resin segment is hydrophilic and tends to extend to the water phase, and the polycarbodiimide compound segment is hydrophobic and tends to be inside the oil phase of the water dispersion particles. Therefore, when the reaction product is emulsified in water, the hydrophilic polyacrylic acid resin segments on the reaction product will be enriched on the surface of the water dispersion; and these polyacrylic acid resin segments, due to their large molecular weight and steric hindrance, will wrap up the polycarbodiimide compound segments to form a polyacrylic acid resin protective layer, so that the polycarbodiimide groups are wrapped inside the water dispersion. When the water-based polycarbodiimide crosslinking agent is used in a water-based coating, since the carbodiimide groups are wrapped, it is difficult to contact and react with the carboxyl groups in the water-based resin in the water-based coating, thereby having a longer usable time.
[0012] The water-based polycarbodiimide crosslinking agent of the present invention is obtained by reacting a polycarbodiimide compound (A) with a polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments, wherein the molar number of the carboxyl group of the polyacrylic resin (B) is 1-20% relative to the molar number of the carbodiimide group in the polycarbodiimide compound (A). The carboxyl group in the polyacrylic resin (B) is insufficient relative to the carbodiimide group in the polycarbodiimide compound (A), and after the two react, the carboxyl group will be completely consumed by the carbodiimide group, so the product after the reaction contains almost no carboxyl group, but contains carbodiimide groups. The present invention is designed that the molar number of the carboxyl group of the polyacrylic resin (B) is 1-20% relative to the molar number of the carbodiimide group in the polycarbodiimide compound (A). If the content of the carboxyl group is too high, the more carbodiimide groups are reacted, the lower the crosslinkable density of the polycarbodiimide compound part in the reaction product (i.e., the number of carbodiimide groups in the reaction product is reduced), resulting in the poor crosslinking effect of the water-based polycarbodiimide crosslinker in the process of forming a coating film when used in a water-based coating. If the content of the carboxyl group is too low, it cannot be ensured that enough polyacrylic acid resin (B) and the polycarbodiimide compound (A) undergo grafting reaction, resulting in the formation of a polyacrylic acid resin protective layer in the water dispersion being limited, so that after the water-based polycarbodiimide crosslinker is used in a water-based coating, the carbodiimide groups of the water-based polycarbodiimide crosslinker are easily in contact with the carboxyl groups in the water-based resin and react, resulting in a shorter usable time.
[0013] As a preferred solution, the average functional number of the carbodiimide group of the polycarbodiimide compound (A) is 2-20. If the average functional number of the carbodiimide group of the polycarbodiimide compound (A) is too large, its chain segment is too long or the volume is too large, which may easily lead to the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments being emulsified in water, and the polyacrylic resin protective layer cannot completely and effectively wrap the carbodiimide group, thereby increasing the possibility of the carbodiimide group contacting the carboxyl group in the water-based resin, resulting in a shortened usable time. If the average functional number of the carbodiimide group of the polycarbodiimide compound (A) is too small, the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments may not have a carbodiimide group, resulting in the water-based polycarbodiimide crosslinker being used in the process of forming a coating film after the water-based coating is used, and the coating film cannot be formed. More preferably, the average functional number of the carbodiimide groups of the polycarbodiimide compound (A) is 2-10.
[0014] As a preferred solution, the polycarbodiimide compound (A) is at least one of an aliphatic polycarbodiimide and an aromatic polycarbodiimide. The carbodiimide groups on the aliphatic polycarbodiimide and the aromatic polycarbodiimide can crosslink with the carboxyl group of the polyacrylic resin (B). Taking into account the speed of the crosslinking reaction, it is more preferred that the polycarbodiimide compound (A) is an aliphatic polycarbodiimide. The reaction speed of the carbodiimide group on the aliphatic polycarbodiimide crosslinking with the carboxyl group is faster than the reaction speed of the carbodiimide group on the aromatic polycarbodiimide crosslinking with the carboxyl group; in addition, the water-based polycarbodiimide crosslinking agent obtained by using the aliphatic polycarbodiimide is faster than the water-based polycarbodiimide crosslinking agent obtained by using the aromatic polycarbodiimide, and is used as a crosslinking agent in a water-based coating. Therefore, it is preferred to use an aliphatic polycarbodiimide as the polycarbodiimide compound (A).
[0015] Further, the raw materials for preparing the polycarbodiimide compound (A) include at least one of aliphatic isocyanate and aromatic isocyanate; the aliphatic isocyanate is at least one of hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and dicyclohexylmethane diisocyanate (HMDI); the aromatic isocyanate is at least one of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI). Preferably, the raw materials for preparing the polycarbodiimide compound (A) are aliphatic isocyanates, so as to facilitate the preparation of aliphatic polycarbodiimide. The above-mentioned raw materials do not represent a limitation on the polycarbodiimide compound (A) of the present invention, and those skilled in the art can select other raw materials to prepare the polycarbodiimide compound (A) according to actual needs.
[0016] As a preferred solution, the solid acid value of the polyacrylic acid resin (B) is 5-61 mg KOH / g. If the acid value is too high, the carboxyl functional number of the polyacrylic acid resin (B) is high, and the reaction with the polycarbodiimide compound (A) is likely to generate some high molecular weight products and gel. If the acid value is too low, it is difficult to ensure that the grafting reaction between the polyacrylic acid resin (B) and the polycarbodiimide compound (A) is complete.
[0017] As a preferred solution, the polyoxyethylene segments in the polyacrylic resin (B) include polyoxyethylene segments, and the weight content of the polyoxyethylene segments in the solid content of the polyacrylic resin (B) is 20-70%. The polyoxyethylene segments are hydrophilic, and the hydrophilicity is provided by the polyoxyethylene segments, thereby improving the water dispersibility of the water-based polycarbodiimide crosslinking agent. The weight content of the polyoxyethylene segments in the solid content of the polyacrylic resin (B) is 20-70%, so that the polyacrylic resin (B) contains enough polyoxyethylene segments to provide hydrophilicity, so that the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments has good hydrophilicity, so that after the reaction product is dispersed in water, a polyacrylic resin protective layer is formed on the surface of the water dispersion particles to isolate the carbodiimide groups and prevent contact with the carboxyl groups of the water-based resin in the water-based coating. If the content of the polyoxyethylene chain segment in the solid content of the polyacrylic resin (B) is too low, it is difficult to form a polyacrylic resin protective layer to isolate the carbodiimide group; if the content of the polyoxyethylene chain segment in the solid content of the polyacrylic resin (B) is too high, the polyacrylic resin (B) will be too hydrophilic, ultimately affecting the water resistance of the water-based polycarbodiimide crosslinker.
[0018] It should be noted that the length of the ethylene oxide segment on the polyacrylic acid resin (B) is not particularly limited, as long as the total weight of the ethylene oxide segment in the solid content of the polyacrylic acid resin (B) is 20-70%. In some embodiments, it should be understood that the polyacrylic acid resin (B) has a ethylene oxide segment, and the ethylene oxide segment can be a whole continuous ethylene oxide segment on the polyacrylic acid resin (B), that is, -(OCH2CH2) n -, the weight content of the continuous polyethylene oxide chain segment in the solid content of the polyacrylic acid resin (B) is 20-70%. Alternatively, the polyacrylic acid resin (B) may have a plurality of discontinuous polyethylene oxide unit chain segments, such as -(OCH2CH2) n1 -、-(OCH2CH2) n2 -、-(OCH2CH2) n3 - etc., the total weight of the plurality of polyethylene oxide unit segments is 20-70% by weight in the solid content of the polyacrylic acid resin (B).
[0019] In some embodiments, the polyoxyalkylene segment in the polyacrylic resin (B) further comprises a polyoxypropylene segment, a polyoxybutylene segment, etc. In some embodiments of the present invention, the polyoxyalkylene segment in the polyacrylic resin (B) may also not comprise a polyoxypropylene segment, a polyoxybutylene segment, and only comprise a polyoxyethylene segment. Those skilled in the art may select according to actual needs.
[0020] As a preferred embodiment, the polyacrylic acid resin (B) is a polymerization product of a monomer (b1), a monomer (b2) and a monomer (b3); the monomer (b1) contains a carboxyl group and an unsaturated double bond; the monomer (b2) contains a polyoxyalkylene chain segment and an unsaturated double bond; the monomer (b3) does not contain a carboxyl group and a polyoxyalkylene chain segment, but contains an unsaturated double bond.
[0021] As a preferred embodiment, the monomer (b1) is at least one of acrylic acid, methacrylic acid, itaconic acid, crotonic acid, β-acryloxypropionic acid, and undecylenic acid; the monomer (b2) is at least one of alkyl polyethylene glycol (meth)acrylate and alkyl polyethylene glycol polypropylene glycol (meth)acrylate; the monomer (b3) is methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, n-butyl methacrylate, n-butyl acrylate, isobutyl methacrylate, isobutyl acrylate, tert-butyl methacrylate, tert-butyl acrylate, 2-ethylhexyl methacrylate, 2-ethylhexyl acrylate, dodecyl methacrylate, dodecyl acrylate, octadecyl methacrylate, octadecyl acrylate, Ester, glycidyl methacrylate, glycidyl acrylate, cyclohexyl methacrylate, cyclohexyl acrylate, 4-tert-butyl cyclohexyl methacrylate, 4-tert-butyl cyclohexyl acrylate, isobornyl methacrylate, isobornyl acrylate, vinyl acetate, vinyl chloride, vinyl dichloride, styrene, p-methylstyrene, m-methylstyrene, α-methylstyrene, methacrylonitrile, acrylonitrile, methacrylamide, acrylamide, divinylbenzene, ethylene glycol dimethacrylate, ethylene glycol diacrylate, polypropylene glycol dimethacrylate, polypropylene glycol diacrylate, 1,4-butanediol dimethacrylate, 1,4-butanediol diacrylate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate at least one. The monomer selection of the above scheme does not represent a limitation on the monomer (b1), monomer (b2) and monomer (b3) of the present invention. Those skilled in the art can also select other monomers (b1), monomers (b2) and monomers (b3) according to the needs of the municipal bureau.
[0022] The present invention also provides a method for preparing any of the above-mentioned water-based polycarbodiimide cross-linking agents, comprising the following steps: adding the polycarbodiimide compound (A) and the polyacrylic resin (B) into a container, reacting until the acid value is zero, and obtaining the water-based polycarbodiimide cross-linking agent.
[0023] The polycarbodiimide compound (A) and the polyacrylic resin (B) react until the acid value is zero, indicating that the carboxyl groups in the polyacrylic resin (B) have been consumed by all reactions. As can be seen from the above, in the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B), the polyacrylic resin segment is hydrophilic and tends to extend to the water phase, and the polycarbodiimide compound segment is hydrophobic and tends to be inside the oil phase of the water dispersion particles. In some schemes, it can be understood that in addition to having carbodiimide groups on the reaction product, there may be polycarbodiimide compounds (A) that do not participate in the reaction (i.e., remaining) in the system after the reaction. According to those skilled in the art, the polycarbodiimide compounds (A) that do not participate in the reaction are more hydrophobic relative to the polycarbodiimide compound segments in the reaction product, and are generally inside the oil phase of the water dispersion particles, so that the carbodiimide groups on the unreacted polycarbodiimide compound (A) are also difficult to contact and react with the carboxyl groups in the water-based resin. In addition, it should be emphasized again that the core of the present invention is that the number of moles of the carboxyl groups of the polyacrylic resin (B) is 1-20% of the number of moles of the carbodiimide groups in the polycarbodiimide compound (A) during the reaction, and the reaction is carried out until the acid value is zero, and there is no restriction on whether there is unreacted (i.e., remaining) polycarbodiimide compound (A) in the system after the reaction.
[0024] As a preferred solution, in the reaction of the polycarbodiimide compound (A) and the polyacrylic resin (B), the reaction temperature is 60-130° C. and the reaction time is 2-10 h.
[0025] In some embodiments, in the preparation method of the water-based polycarbodiimide crosslinker, an organic solvent can also be added to the container. By adding an organic solvent to the reaction of the polycarbodiimide compound (A) and the polyacrylic resin (B), the reaction is facilitated. Preferably, the boiling point of the organic solvent is ≥60°C. If the boiling point of the organic solvent is too low, the organic solvent will volatilize seriously. Preferably, the amount of the organic solvent added is 0-10% of the total weight of the water-based polycarbodiimide crosslinker. If the amount of organic solvent added is too much, it is not environmentally friendly and leads to an increase in the VOC content in the water-based polycarbodiimide crosslinker. Preferably, the organic solvent is preferably aromatic hydrocarbons, ketones, alcohol ethers, ethers, esters, etc.
[0026] In other embodiments, the organic solvent may not be added in the preparation method of the water-based polycarbodiimide crosslinking agent. Of course, those skilled in the art may choose to add or not add the organic solvent according to actual needs.
[0027] In some embodiments, in the preparation method of the water-based polycarbodiimide crosslinker, after the reaction is completed, water is added for emulsification to obtain the water-based polycarbodiimide crosslinker. After the reaction of the polycarbodiimide compound (A) and the polyacrylic acid resin (B) containing carboxyl and polyoxyalkylene segments is completed, water is added for emulsification so that the water-based polycarbodiimide crosslinker forms an aqueous dispersion, so that the hydrophilic polyacrylic acid resin segment portion will be enriched on the surface of the aqueous dispersion to form a polyacrylic acid resin protective layer, which wraps and isolates the carbodiimide group. The amount of water added is 50-80% of the total weight of the water-based polycarbodiimide crosslinker; if the amount of water added is too little, the viscosity of the water-based polycarbodiimide crosslinker will be too large; if the amount of water added is too little, the effective ingredient content of the water-based polycarbodiimide crosslinker will be low.
[0028] In other embodiments, in the preparation method of the water-based polycarbodiimide crosslinker, after the reaction is completed, an external emulsifier can be added first, and then water can be added for emulsification to obtain the water-based polycarbodiimide crosslinker. The amount of the external emulsifier added is 0-5% of the total weight of the water-based polycarbodiimide crosslinker; after the reaction of the polycarbodiimide compound (A) and the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments is completed, the external emulsifier is first added, and then water is added for emulsification to improve the emulsification effect, so that the water-based polycarbodiimide crosslinker forms a water dispersion and is effectively dispersed on the surface of the water dispersion. The present invention has no special restrictions on the added external emulsifier, and is preferably an ionic or non-ionic emulsifier. Of course, those skilled in the art can choose to add or not add the external emulsifier according to actual needs.
[0029] The present invention further provides the use of any of the above-mentioned water-based polycarbodiimide cross-linking agents:
[0030] As an application, the present invention provides a cross-linkable composition, comprising the water-based polycarbodiimide cross-linking agent and a carboxyl-containing water-based resin.
[0031] As another application, specifically, the application of any of the above-mentioned polycarbodiimide crosslinking agents in the preparation of water-based coatings. The water-based coating comprises the crosslinkable composition (i.e., comprising any of the above-mentioned water-based polycarbodiimide crosslinking agents and a carboxyl-containing water-based resin). Before the construction of the water-based coating, since it is in an aqueous phase state, most of the carbodiimide groups are wrapped inside the dispersion particles of the water-based polycarbodiimide crosslinking agent, and the particle surface of the water-based polycarbodiimide crosslinking agent is a polyacrylic resin layer with steric hindrance. At this time, the carbodiimide groups are difficult to contact with the carboxyl groups in the water-based resin, and the reaction will be very slow, thereby having a longer service life. In the process of the water-based coating being dried to form a coating film, as the water evaporates, the carbodiimide groups in the water-based polycarbodiimide crosslinking agent will undergo a crosslinking reaction with the carboxyl groups in the carboxyl-containing water-based resin to form a crosslinking network, thereby providing the coating film with better chemical properties.
[0032] As a preferred solution, the water-based coating comprises the following components in parts by weight: 2-10 parts of any of the above-mentioned water-based polycarbodiimide cross-linking agents and 85 parts of a carboxyl-containing water-based resin.
[0033] Furthermore, the water-based paint further comprises other additives, and the weight portion of the other additives in the water-based paint is 1-14 parts. By adding other additives, the performance of the water-based paint is improved. Preferably, the weight portion of the other additives in the water-based paint is 3-8 parts.
[0034] As a preferred solution, the other additives include one or more of a defoamer, a leveling agent, a cosolvent or a thickener. The weight portion of the defoamer in the water-based paint is 0.1-1 part; the weight portion of the leveling agent in the water-based paint is 0.1-1 part; the weight portion of the cosolvent in the water-based paint is 1-10 parts; the weight portion of the thickener in the water-based paint is 0.1-2 parts. The defoamer eliminates the bubbles generated during the stirring process and the bubbles generated during the reaction process; the leveling agent acts on the interface between the water-based paint liquid and the air to improve the flatness of the paint film surface and prevent defects such as Bénard vortices; the cosolvent improves the film-forming properties of the water-based paint, establishes a volatilization gradient of the water-based paint, and improves the surface effect of the film; the thickener adjusts the rheological properties of the water-based paint to improve the paint's anti-sagging, anti-splashing and other properties.
[0035] As a preferred solution, the defoamer is at least one of a polysiloxane defoamer and a mineral oil defoamer; the leveling agent is at least one of a polysiloxane leveling agent and an acrylic leveling agent; the cosolvent is at least one of ethylene glycol butyl ether, propylene glycol butyl ether, diethylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether; the thickener is at least one of a polyurethane thickener, an alkali swellable acrylic thickener, and bentonite. The above-mentioned defoamers, leveling agents, cosolvents, and thickeners do not represent limitations on the present invention, and those skilled in the art may also select other types of defoamers, leveling agents, cosolvents, and thickeners according to actual needs.
[0036] The present invention also provides a method for preparing the water-based paint, comprising the following steps: uniformly mixing the components to obtain the water-based paint.
[0037] As another application, the present invention provides a product coated with the water-based paint, which is formed by spraying the water-based paint including the water-based polycarbodiimide crosslinking agent on the surface of a substrate.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The water-based polycarbodiimide cross-linking agent of the present invention can be applied to water-based coatings and can be stored together with the carboxyl-containing water-based resin in the water-based coatings for a long time, so that the water-based coatings have a very long usable time, and the coating film formed by the water-based coatings has very good water resistance and chemical resistance, thereby improving the performance of the water-based coatings.
[0040] The present invention obtains the water-based polycarbodiimide crosslinking agent by reacting the polycarbodiimide compound (A) with the polyacrylic resin (B) containing carboxyl and polyoxyalkylene segments, so that the hydrophilic polyoxyalkylene segments are introduced into the polycarbodiimide compound (A) through the polyacrylic resin (B), thereby improving the water dispersibility of the water-based polycarbodiimide crosslinking agent. In addition, after the reaction product of the polycarbodiimide compound (A) and the polyacrylic resin (B) is emulsified in water, the polyacrylic resin part on the reaction product will be enriched on the surface of the dispersion to form a polyacrylic resin protective layer, isolating and encapsulating the carbodiimide group, so that the carbodiimide group is encapsulated inside the water dispersion, so that the carbodiimide group on the water-based polycarbodiimide crosslinking agent is difficult to contact with the carboxyl group in the water-based resin in the water dispersion and react, so it has a long usable time. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.
[0042] Example 1
[0043] This embodiment provides a water-based polycarbodiimide cross-linking agent C1, which is obtained by reacting a polycarbodiimide compound A1 and a polyacrylic acid resin B1.
[0044] The water-based polycarbodiimide crosslinking agent C1 of this embodiment is prepared by the following process:
[0045] (1) Preparation of polycarbodiimide compound A1:
[0046] The reaction flask was filled with nitrogen, and 1049.4 g of dicyclohexylmethane diisocyanate, 198.3 g of butyl isocyanate, and 12.6 g of 1-methylphosphine-1-oxide (MPO) were added. The mixture was heated to 160° C. and reacted until the NCO value reached zero to obtain polycarbodiimide compound A1.
[0047] The theoretical average carbodiimide functional number of the polycarbodiimide compound A1 is 5.
[0048] (2) Preparation of polyacrylic acid resin B1:
[0049] Nitrogen was passed through the reaction flask, 300.0 g of dipropylene glycol dimethyl ether was added, and the reaction flask was heated to 140° C. A mixture of 331.6 g of MPEG (1000) MA (methoxy polyethylene glycol methacrylate, molecular weight 1000), 326.2 g of n-butyl acrylate, 18.2 g of acrylic acid, and 24.0 g of di-tert-butyl peroxide was dripped into the reaction flask, and the reaction was carried out for 5 hours, and then the temperature was kept at 140° C. for 3 hours to obtain polyacrylic resin B1.
[0050] The solid acid value of the polyacrylic acid resin B1 is Av=20.2 mg KOH / g, and the weight of the polyethylene oxide chain segment accounts for about 41% of the solid weight of the polyacrylic acid resin B1.
[0051] (3) Preparation of water-based polycarbodiimide crosslinking agent C1:
[0052] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A1 (containing 0.481 mol of carbodiimide groups) and 100.0 g of polyacrylic resin B1 (containing 0.0253 mol of carboxyl groups) were added, and heated to 75°C for 8 h. At this time, the acid value was zero. 225.0 g of deionized water was added under high-speed stirring to obtain a milky liquid, i.e., water-based polycarbodiimide crosslinker C1, with a solid content of 40%.
[0053] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A1 modified by the carboxyl groups in the polyacrylic resin B1 was 5.3%.
[0054] Example 2
[0055] This embodiment provides a water-based polycarbodiimide crosslinking agent C2, which is obtained by reacting the polycarbodiimide compound A1 of Example 1 and the polyacrylic acid resin B2.
[0056] The water-based polycarbodiimide crosslinking agent C2 of this embodiment is prepared by the following process:
[0057] (1) Take the polycarbodiimide compound A1 of Example 1;
[0058] (2) Preparation of polyacrylic acid resin B2:
[0059] Nitrogen was passed through the reaction flask, 300.0 g of dipropylene glycol dimethyl ether was added, and the reaction flask was heated to 150° C. A mixture of 331.6 g of MPEG (1000) MA (methoxy polyethylene glycol methacrylate, molecular weight 1000), 290.2 g of n-butyl acrylate, 54.2 g of acrylic acid, and 24.0 g of di-tert-amyl peroxide was dripped into the reaction flask, and the reaction was carried out for 5 hours, and then the temperature was kept at 150° C. for 3 hours to obtain polyacrylic resin B2.
[0060] The solid acid value of the polyacrylic acid resin B2 is Av=40.3 mg KOH / g, and the weight of the polyethylene oxide chain segment accounts for about 41% of the solid weight of the polyacrylic acid resin B2.
[0061] (3) Preparation of water-based polycarbodiimide crosslinking agent C2:
[0062] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A1 (containing 0.481 mol of carbodiimide groups) and 125.0 g of polyacrylic resin B2 (containing 0.0941 mol of carboxyl groups) were added, and heated to 75°C for 8 hours. At this time, the acid value was zero. 244.0 g of deionized water was added under high-speed stirring to obtain a milky liquid, i.e., an aqueous polycarbodiimide crosslinker C2, with a solid content of 40%.
[0063] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A1 modified by the carboxyl groups in the polyacrylic resin B2 was 19.6%.
[0064] Example 3
[0065] This embodiment provides a water-based polycarbodiimide crosslinking agent C3, which is obtained by reacting the polycarbodiimide compound A1 of Example 1 and the polyacrylic acid resin B3.
[0066] The water-based polycarbodiimide crosslinking agent C3 of this embodiment is prepared by the following process:
[0067] (1) Take the polycarbodiimide compound A1 of Example 1;
[0068] (2) Preparation of polyacrylic acid resin B3:
[0069] Nitrogen was passed through the reaction flask, 300.0 g of dipropylene glycol dimethyl ether was added, and the flask was heated to 80°C. A mixture of 337.4 g of MPEG (1000) MA (methoxy polyethylene glycol methacrylate, molecular weight 1000), 345.5 g of n-butyl acrylate, 4.89 g of acrylic acid, and 12.2 g of azobisisobutyronitrile (AIBN) was dripped into the reaction flask. The reaction was carried out for 5 hours, and then the temperature was kept at 80°C for 3 hours to obtain polyacrylic resin B3.
[0070] The solid acid value of the polyacrylic acid resin B3 is Av=5.4 mg KOH / g, and the weight of the polyethylene oxide chain segment accounts for about 41% of the solid weight of the polyacrylic acid resin B3.
[0071] (3) Preparation of water-based polycarbodiimide crosslinking agent C3:
[0072] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A1 (containing 0.481 mol of carbodiimide groups) and 80.0 g of polyacrylic resin B3 (containing 0.0054 mol of carboxyl groups) were added, and heated to 75°C for 8 hours. At this time, the acid value was zero. 210.0 g of deionized water was added under high-speed stirring to obtain a milky liquid, i.e., an aqueous polycarbodiimide crosslinker C3, with a solid content of 40%.
[0073] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A1 modified by the carboxyl groups in the polyacrylic resin B3 was 1.1%.
[0074] Example 4
[0075] This embodiment provides a water-based polycarbodiimide crosslinking agent C4, which is obtained by reacting the polycarbodiimide compound A1 of Example 1 and the polyacrylic acid resin B4.
[0076] The water-based polycarbodiimide crosslinking agent C4 of this embodiment is prepared by the following process:
[0077] (1) Take the polycarbodiimide compound A1 of Example 1.
[0078] (2) Preparation of polyacrylic acid resin B4:
[0079] Nitrogen was passed through the reaction flask, 300.0 g of dipropylene glycol dimethyl ether was added, and the flask was heated to 140°C. A mixture of 516.6 g of MPEG (2000) MA (methoxy polyethylene glycol methacrylate, 2000 molecular weight), 141.2 g of n-butyl acrylate, 18.2 g of acrylic acid, and 24.0 g of di-tert-butyl peroxide was dripped into the reaction flask. The reaction was carried out for 5 hours, and then the temperature was kept at 140°C for 3 hours to obtain polyacrylic resin B4.
[0080] The solid acid value of the polyacrylic acid resin B4 is Av=20.2 mg KOH / g, and the weight of the polyethylene oxide chain segment accounts for about 69% of the solid weight of the polyacrylic acid resin B4.
[0081] (3) Preparation of water-based polycarbodiimide crosslinking agent C4:
[0082] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A1 (containing 0.481 mol of carbodiimide groups) and 100.0 g of polyacrylic resin B4 (containing 0.0253 mol of carboxyl groups) were added, and heated to 75°C for 8 h. At this time, the acid value was zero. 225.0 g of deionized water was added under high-speed stirring to obtain a milky white liquid, i.e., water-based polycarbodiimide crosslinker C4, with a solid content of 40%.
[0083] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A1 modified by the carboxyl groups in the polyacrylic resin B4 was 5.3%.
[0084] Example 5
[0085] This embodiment provides a water-based polycarbodiimide crosslinking agent C5, which is obtained by reacting the polycarbodiimide compound A1 of Example 1 and the polyacrylic acid resin B5.
[0086] The water-based polycarbodiimide crosslinking agent C5 of this embodiment is prepared by the following process:
[0087] (1) Take the polycarbodiimide compound A1 of Example 1.
[0088] (2) Preparation of polyacrylic acid resin B5:
[0089] Nitrogen was passed through the reaction flask, 300.0 g of dipropylene glycol dimethyl ether was added, and the flask was heated to 140° C. A mixture of 188.2 g of MPEG (600) MA (methoxy polyethylene glycol methacrylate, 600 molecular weight), 469.6 g of n-butyl acrylate, 18.2 g of acrylic acid, and 24.0 g of di-tert-butyl peroxide was dripped into the reaction flask, and the reaction was carried out for 5 hours, and then the temperature was kept at 140° C. for 3 hours to obtain polyacrylic resin B5.
[0090] The solid acid value of the polyacrylic acid resin B5 is Av=20.2 mg KOH / g, and the weight of the polyethylene oxide chain segment accounts for about 21% of the solid weight of the polyacrylic acid resin B5.
[0091] (3) Preparation of water-based polycarbodiimide crosslinking agent C5:
[0092] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A1 (containing 0.481 mol of carbodiimide groups) and 100.0 g of polyacrylic resin B5 (containing 0.0253 mol of carboxyl groups) were added, and heated to 75°C for 8 h. At this time, the acid value was zero. 225.0 g of deionized water was added under high-speed stirring to obtain a milky liquid, i.e., a water-based polycarbodiimide crosslinker C5, with a solid content of 40%.
[0093] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A1 modified by the carboxyl groups in the polyacrylic resin B5 was 5.3%.
[0094] Example 6
[0095] This embodiment provides a water-based polycarbodiimide crosslinking agent C6, which is obtained by reacting a polycarbodiimide compound A2 with the polyacrylic acid resin B1 of Example 1.
[0096] The water-based polycarbodiimide crosslinking agent C6 of this embodiment is prepared by the following process:
[0097] (1) Preparation of polycarbodiimide compound A2:
[0098] The reaction flask was filled with nitrogen, and 2098.8 g of dicyclohexylmethane diisocyanate, 198.3 g of butyl isocyanate, and 23.0 g of 1-methylphosphine-1-oxide (MPO) were added. The mixture was heated to 160° C. and reacted until the NCO value reached zero to obtain polycarbodiimide compound A2.
[0099] The theoretical average carbodiimide functional number of the polycarbodiimide compound A2 is 9.
[0100] (2) Take the polyacrylic acid resin B1 of Example 1.
[0101] (3) Preparation of water-based polycarbodiimide crosslinking agent C6:
[0102] A reaction flask was filled with nitrogen, 100.0 g of polycarbodiimide compound A2 (containing 0.468 mol of carbodiimide groups) and 100.0 g of polyacrylic resin B1 (containing 0.0253 mol of carboxyl groups) were added, and the mixture was heated to 75°C for 8 h, at which time the acid value was zero. 225.0 g of deionized water was added under high-speed stirring to obtain a milky white liquid, i.e., water-based polycarbodiimide crosslinker C6, with a solid content of 40%.
[0103] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A2 modified by the carboxyl groups in the polyacrylic resin B1 was 5.4%.
[0104] Example 7
[0105] This embodiment provides a water-based polycarbodiimide crosslinking agent C7, which is obtained by reacting a polycarbodiimide compound A3 with the polyacrylic acid resin B1 of Example 1.
[0106] The water-based polycarbodiimide crosslinking agent C7 of this embodiment is prepared by the following process:
[0107] (1) Preparation of polycarbodiimide compound A3:
[0108] The reaction flask was filled with nitrogen, and 262.4 g of dicyclohexylmethane diisocyanate, 198.3 g of butyl isocyanate, and 4.7 g of 1-methylphosphine-1-oxide (MPO) were added. The mixture was heated to 160° C. and reacted until the NCO value reached zero to obtain polycarbodiimide compound A3.
[0109] The theoretical average carbodiimide functional number of the polycarbodiimide compound A3 is 2.
[0110] (2) Take the polyacrylic acid resin B1 of Example 1.
[0111] (3) Preparation of water-based polycarbodiimide crosslinking agent C7:
[0112] A reaction flask was filled with nitrogen, and 100.0 g of polycarbodiimide compound A3 (containing 0.530 mol of carbodiimide groups) and 100.0 g of polyacrylic resin B1 (containing 0.0253 mol of carboxyl groups) were added, and heated to 75°C for 8 h. At this time, the acid value was zero. 225.0 g of deionized water was added under high-speed stirring to obtain a milky liquid, i.e., water-based polycarbodiimide crosslinker C7, with a solid content of 40%.
[0113] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A3 modified by the carboxyl groups in the polyacrylic resin B1 was 4.8%.
[0114] Example 8
[0115] This embodiment provides a water-based polycarbodiimide crosslinking agent C8, which is obtained by reacting a polycarbodiimide compound A4 with the polyacrylic acid resin B1 of Example 1.
[0116] The water-based polycarbodiimide crosslinking agent C8 of this embodiment is prepared by the following process:
[0117] (1) Preparation of polycarbodiimide compound A4:
[0118] A reaction flask was filled with nitrogen, 889.3 g of isophorone diisocyanate, 125.2 g of cyclohexyl isocyanate, and 10.3 g of 1-methylphosphine-1-oxide (MPO) were added, and the mixture was heated to 160° C. and reacted until the NCO value reached 5.0%. The mixture was cooled to 130° C., 750.0 g of polyethylene glycol monomethyl ether (molecular weight 750) was added, and the reaction was continued until the NCO value reached zero to obtain polycarbodiimide compound A4.
[0119] The theoretical average carbodiimide functional number of the polycarbodiimide compound A3 is 4.
[0120] (2) Take the polyacrylic acid resin B1 of Example 1.
[0121] (3) Preparation of water-based polycarbodiimide crosslinking agent C8:
[0122] A reaction flask was filled with nitrogen, 100.0 g of polycarbodiimide A4 (containing 0.250 mol of carbodiimide groups) and 100.0 g of polyacrylic acid resin B1 (containing 0.0253 mol of carboxyl groups) were added, and the mixture was heated to 75°C for 8 h. At this time, the acid value was zero. The solvent was removed by vacuum, and 40.0 g of a 10% aqueous solution of sodium dodecyl sulfate was added, and the mixture was stirred until uniform. 229.0 g of deionized water was added under high-speed stirring to obtain a milky white liquid, i.e., an aqueous polycarbodiimide crosslinker C8, with a solid content of 40%.
[0123] The molar ratio of the carbodiimide groups in the polycarbodiimide compound A4 modified by the carboxyl groups in the polyacrylic resin B1 was 10.1%.
[0124] Comparative Example 1
[0125] This comparative example provides a water-based polycarbodiimide crosslinking agent C9, which is modified directly with polyethylene glycol monomethyl ether MPEG instead of using polyacrylic acid resin B for modification compared to Examples 1-8.
[0126] The water-based polycarbodiimide crosslinking agent C9 of this comparative example is prepared by the following process:
[0127] A nitrogen atmosphere was passed through the reaction flask, and 889.3 g of dicyclohexylmethane diisocyanate, 125.2 g of butyl isocyanate, and 10.3 g of 1-methylphosphine-1-oxide (MPO) were added, and the mixture was heated to 160°C and reacted until the NCO value reached 5.0%. The mixture was cooled to 130°C, and 750.0 g of MPEG750 (polyethylene glycol monomethyl ether, 750 molecular weight) was added and reacted until the NCO value reached zero. 1065.9 g of deionized water was added under high-speed stirring to obtain a translucent yellow liquid, i.e., an aqueous polycarbodiimide crosslinker C9, with a solid content of 40%.
[0128] Example 9
[0129] This embodiment provides a crosslinkable composition, including any of the water-based polycarbodiimide crosslinking agents of embodiments 1-8, and a water-based polyurethane dispersion (i.e., a carboxyl-containing water-based resin), wherein the weight parts of the water-based polycarbodiimide crosslinking agent are 8 parts, and the weight parts of the water-based polyurethane dispersion are 85 parts.
[0130] Example 10
[0131] The present embodiment provides a water-based coating, comprising the following components in parts by weight: 8 parts of a water-based polycarbodiimide cross-linking agent of any one of Embodiments 1-8; 85 parts of a water-based polyurethane dispersion; 0.2 parts of a defoaming agent; 0.3 parts of a leveling agent; 4 parts of a cosolvent; 0.5 parts of a thickener; and 10 parts of water.
[0132] The preparation method of the water-based paint of this embodiment includes the following steps: mixing the components evenly to obtain the water-based paint.
[0133] Embodiment 11
[0134] This embodiment provides a product coated with the water-based coating of Embodiment 10.
[0135] The water-based coating in Example 10, i.e., the water-based coating formed by the water-based polycarbodiimide crosslinking agent in Examples 1-8, was sprayed on the surface of the plastic substrate to form a coating film with a thickness of 23±3 μm on the surface of the plastic substrate.
[0136] Performance Testing
[0137] The performance of the water-based polycarbodiimide crosslinking agent of Examples 1-8 and Comparative Example 1 was tested: the process is as follows:
[0138] The water-based polycarbodiimide crosslinking agents C1-C9 of Examples 1-8 and Comparative Example 1, and the commercial water-based polycarbodiimide crosslinking agent OS-8000 (Guangzhou Guanzhi New Materials, solid content: 40%, not modified with polyacrylic acid resin) were respectively mixed with a commercial water-based polyurethane dispersion (trade name PU-6081, Guangzhou Guanzhi New Materials, solid content: 38%) to prepare water-based coatings 1-10 according to the formula in Table 1.
[0139] Table 1 Water-based coating formulation
[0140]
[0141]
[0142] The following performance tests were performed on water-based coatings 1-10:
[0143] Water resistance test: spray the freshly prepared water-based paint on the plastic PC substrate with a film thickness of 23±3μm, bake at 70℃ for 2h, and then keep at room temperature overnight. Soak the plastic plate in room temperature water and observe the whitening and bubbling of the coating after 24h. Score 1-5 points, with 5 points being the best.
[0144] Alcohol resistance test: spray the freshly prepared water-based paint on the plastic PC substrate with a film thickness of 23±3μm, bake at 70℃ for 2h, and then keep at room temperature overnight. Soak the plastic plate in ethanol (50% aqueous solution) and observe the whitening and bubbling of the coating after 1h. Score 1-5 points, with 5 points being the best.
[0145] Usable time test: Test the water resistance and alcohol resistance of the prepared water-based paint every other day. If the water resistance and alcohol resistance have significantly decreased, it means that the usable time has expired. (Among them, significant decrease means that the water resistance or alcohol resistance score has dropped by 2 levels compared with the initial score; for example, if the water resistance (or alcohol resistance) score of the water-based paint was originally 4 points, and the water resistance (or alcohol resistance) score tested after a certain period of time is only 2 points, it is considered that the water resistance (or alcohol resistance) has significantly decreased).
[0146] The test results are shown in the following table:
[0147] Table 2 Test results of water-based coatings
[0148]
[0149]
[0150] The water-based coating formula in Table 1 and the performance test results in Table 2 show that the water-based coating 1-8 to which the water-based polycarbodiimide crosslinking agent C1-C8 of Examples 1-8 of the present invention is added has a longer usable time. This is because the water-based polycarbodiimide crosslinking agent C1-C8 of Examples 1-8 is obtained by modifying the polycarbodiimide compound (A) with a hydrophilic polyacrylic resin (B) with large steric hindrance, so that a polyacrylic resin protective layer is formed on the surface of the water dispersion particles of the water-based polycarbodiimide crosslinking agent C1-C8 of Examples 1-8, which wraps and isolates the carbodiimide groups; after the water-based polycarbodiimide crosslinking agent C1-C8 of Examples 1-8 and the carboxyl-containing water-based resin (such as water-based polyurethane dispersion) are configured into the water-based coating 1-8 according to the formula, the carbodiimide groups on the water-based polycarbodiimide crosslinking agent C1-C8 are more difficult to contact the carboxyl-containing water-based resin, and thus have a much longer usable time.
[0151] The usable time of the water-based coating 9 to which the water-based polycarbodiimide crosslinker C9 of comparative example 1 is added, and the water-based coating 10 to which the water-based polycarbodiimide crosslinker OS-8000 is added is much shorter than that of the water-based coatings 1-8 of the present invention. This is because the water-based polycarbodiimide crosslinker C9 of comparative example 1 and the water-based polycarbodiimide crosslinker OS-8000 are not modified with polyacrylic acid resin, and no polyacrylic acid resin protective layer is formed on the surface of the water dispersion particles to wrap and isolate the carbodiimide groups; after the water-based polycarbodiimide crosslinker C9 and the water-based polycarbodiimide crosslinker OS-8000 of comparative example 1 are respectively formulated into water-based coatings 9-10 with carboxyl-containing water-based resins (such as water-based polyurethane dispersions) according to the formula, the carbodiimide groups are easily in contact with the carboxyl-containing water-based resins to undergo crosslinking, and thus the usable time is shorter.
[0152] Compared with the prior art, the water-based polycarbodiimide cross-linking agent of the present invention is applied to water-based coatings and can be stored together with the carboxyl-containing water-based resin in the water-based coatings for a long time, so that the water-based coatings have a very long usable time, and the coating film formed by the water-based coatings has very good water resistance and chemical resistance, thereby improving the performance of the water-based coatings.
[0153] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.
Claims
1. A water-based polycarbodiimide crosslinking agent, characterized in that: Obtained by the reaction of a polycarbodiimide compound (A) and a polyacrylic acid resin (B); wherein: The average carbodiimide group functional number of the polycarbodiimide compound (A) is 2-20; The polyacrylic acid resin (B) contains carboxyl and polyoxyalkylene segments; the solid acid value of the polyacrylic acid resin (B) is 5-61 mg KOH / g; The number of moles of the carboxyl group of the polyacrylic resin (B) is 1 to 20% of the number of moles of the carbodiimide group in the polycarbodiimide compound (A).
2. The water-based polycarbodiimide crosslinking agent according to claim 1, characterized in that: The polycarbodiimide compound (A) is at least one of an aliphatic polycarbodiimide and an aromatic polycarbodiimide.
3. The water-based polycarbodiimide crosslinking agent according to claim 1, characterized in that: The polyoxyalkylene segment in the polyacrylic resin (B) includes a polyoxyethylene segment, and the weight content of the polyoxyethylene segment in the solid content of the polyacrylic resin (B) is 20-70%.
4. The water-based polycarbodiimide crosslinking agent according to claim 3, characterized in that: The polyacrylic acid resin (B) is a polymerization product of monomer (b1), monomer (b2) and monomer (b3); The monomer (b1) contains a carboxyl group and an unsaturated double bond; the monomer (b2) contains a polyoxyalkylene chain segment and an unsaturated double bond; and the monomer (b3) does not contain a carboxyl group and a polyoxyalkylene chain segment but contains an unsaturated double bond.
5. A method for preparing the water-based polycarbodiimide crosslinking agent according to any one of claims 1 to 4, characterized in that: The polycarbodiimide compound (A) and the polyacrylic resin (B) are added into a container and reacted until the acid value reaches zero to obtain the water-based polycarbodiimide crosslinking agent.
6. The method for preparing the water-based polycarbodiimide crosslinking agent according to claim 5, characterized in that: The reaction temperature is 60-130°C and the reaction time is 2-10h.
7. The method for preparing the water-based polycarbodiimide crosslinking agent according to claim 6, characterized in that: After the reaction, water is added for emulsification to obtain the water-based polycarbodiimide cross-linking agent; wherein the amount of water added is 50-80% of the total weight of the water-based polycarbodiimide cross-linking agent.
8. Use of the water-based polycarbodiimide crosslinking agent according to any one of claims 1 to 4 in the preparation of water-based coatings.