Metal-modified Al₂O₃ aldol condensation catalyst, its preparation and application
By loading active components and additives onto a metal-modified Al2O3 support, stable acid-base active sites are formed, solving the problem of catalyst susceptibility to hydrolysis, improving the selectivity and conversion rate of methyl methacrylate, and realizing the industrial application of green production.
Patent Information
- Application Number
- CN202211514279.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-11-29
AI Technical Summary
Existing catalysts are prone to hydrolysis in the aldol condensation reaction of formaldehyde and methyl propionate, resulting in low activity and poor selectivity, making them difficult to apply industrially.
Metal-modified Al2O3 support is used. By loading active components such as metals Nb, Mg, Cs, and K and promoters such as P, Ag, V, Fe, Cu, and La onto Al2O3, a stable Al-OM structure is formed, which improves the physical and mechanical properties and acid-base active sites of the catalyst.
This enhanced the catalyst's activity and lifespan, improved the selectivity and conversion rate of methyl methacrylate, solved the hydrolysis problem, and enabled the industrial application of green production of methyl methacrylate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a metal-modified Al2O3 aldol condensation catalyst and its preparation and application, specifically to the preparation of a modified Al2O3 support catalyst for aldol condensation and its method for condensing formaldehyde and methyl propionate in a mixed solution (or an aqueous mixed solution) to prepare methyl methacrylate. Background Technology
[0002] Methyl methacrylate (MMA) is an important organic chemical raw material, mainly used in the production of plexiglass (polymethyl methacrylate, PMMA). It is also used in the manufacture of other resins, as an impact modifier for PVC plastics, coatings, impregnating agents for wood and cork, impregnating agents for motor coils, and insulating potting materials, among other industrial applications. In 2020, the global MMA market reached 51.4 billion yuan, and it is projected to reach 64.9 billion yuan by 2026, with a compound annual growth rate (CAGR) of 3.4%.
[0003] From a raw material perspective, MMA production methods can be categorized into: the acetone cyanohydrin (ACH) method, and C2, C3, and C4 routes. Currently, the main domestic MMA production process is the ACH method, which is costly and highly polluting. The Alpha method, however, is a new green production route, primarily consisting of two steps: first, ethylene is carbonylated to synthesize methyl propionate; then, methyl propionate and formaldehyde are condensed together to synthesize MMA. This method features readily available and safe raw materials, and is environmentally friendly and pollution-free. This series of catalysts has also been extensively studied, as reported in patents CN201410784248, CN201210276200, CN201810925782, CN201910368812, CN201110212068, EP0710643, USPat.No.4,618,709, and USPat.No.4,956,493. However, the formaldehyde source used in this series of catalysts is mostly obtained by dissolving methyl acetal, trioxymethylene or paraoxymethylene in methanol. However, water is inevitably generated in the aldol condensation reaction, which easily causes hydrolysis of raw materials and products and deactivation of catalysts, resulting in problems such as low catalyst activity and poor selectivity. Although some studies have proposed modifying the support or adding a small amount of water-resistant additives to improve the water resistance of the catalyst, the effect is not very obvious, so it has been difficult to promote its industrial application. Summary of the Invention
[0004] The main technical problem solved by this invention is to provide a method for preparing a catalyst for aldol condensation reaction using metal-modified Al2O3 and for condensing it in a mixed solution (or aqueous mixed solution) of formaldehyde and methyl propionate to prepare methyl methacrylate.
[0005] A metal-modified Al₂O₃ aldehyde condensation catalyst, its preparation and application, specifically:
[0006] Preparation of metal-modified Al₂O₃ aldol condensation catalyst:
[0007] The Al2O3 support is modified by adding one or more precursor solutions of Si, Zr, and Ti, stirring at 25-100℃ for 2-24 hours, and then evaporating the moisture and drying. Alternatively, Al2O3 can be mechanically mixed with one or more of diatomaceous earth and kaolin. The active component X is one or more precursor salts of metals Nb, Mg, Cs, and K, with a content of 1-50 wt% (based on metal oxides) relative to the support. The auxiliary agent Z is one or more precursor salts of metals P, Ag, V, Fe, Cu, and La, with a content of 0.05-5 wt% (based on metal oxides) relative to the support. Finally, the active component X and the auxiliary agent Z are loaded onto the modified support M-Al2O3 by impregnation.
[0008] The active component X includes, but is not limited to, one or more of the following: carbonate, acetate, and citrate of Mg; oxalate of Nb; acetate, carbonate, sulfate, and nitrate of Cs; and citrate, carbonate, bicarbonate, and nitrate of K.
[0009] The auxiliary agent Z includes, but is not limited to, one or more of the following: diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate trihydrate, potassium phosphate, silver nitrate, silver carbonate, ammonium metavanadate, ferric phosphate dihydrate, ferric nitrate nonahydrate, ferric citrate, basic copper carbonate, copper citrate, copper nitrate hydrate, copper nitrate trihydrate, copper acetate, lanthanum nitrate, and lanthanum nitrate hexahydrate.
[0010] In the catalyst, the modifying agent M accounts for 1-30 wt% (relative to the Al2O3 support); the active component X and the auxiliary agent Z account for 1-50 wt% and 0.05-5 wt% (both calculated as metal oxides) relative to the modified support, respectively.
[0011] In the catalyst, the modified support M-Al2O3 is added to the prepared mixed solution of active component and auxiliary agent, mixed thoroughly and dried, and then calcined in air at 300-800℃ for 3-10h. This is the method for preparing the modified support for aldol condensation reaction catalyst.
[0012] The catalyst is applied in a fixed-bed reactor. The specific reaction process is as follows: The catalyst (20-60 mesh after molding) is filled into the middle section of the fixed-bed reactor, while the upper and lower sections are filled with quartz sand. The raw material is a mixed solution of formaldehyde and methyl propionate or an aqueous mixed solution thereof. The carrier gas is N2, and the molar ratio of methyl propionate to formaldehyde is 1:(1-3). The reaction is carried out at 200-450℃ under normal pressure, with an LHSV of 0.1-3 h. -1 The product is a mixed solution containing methyl methacrylate and methacrylic acid.
[0013] The reactions involved in this invention can be represented by the following reaction equations:
[0014] CH3OH + 1 / 2O2 = HCHO + H2O
[0015]
[0016] Beneficial technical effects of the present invention:
[0017] The prepared catalyst has suitable acid and base active sites. The modified M-Al2O3 support can form a stable Al-OM framework during calcination, which is beneficial to enhancing the physical and mechanical properties of the catalyst. It also has a large specific surface area and pore size, which is beneficial to slowing down the loss of active components of the catalyst and its anti-carbon deposition ability, thereby improving the activity and lifespan of the catalyst. Detailed Implementation
[0018] The preferred embodiments of the present invention will be described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.
[0019] Example 1
[0020] Dissolve 0.24 g of titanium tetrachloride in 15 ml of deionized water, and denote this as solution A. Weigh 10 g of the support γ-Al2O3 and add it to solution A. Stir continuously at 60 °C for 2 h under magnetic stirring. Then dry at 120 °C for 12 h. After drying, calcine the solid at 550 °C in air for 4 h. The product obtained is the 1 wt% Ti-modified γ-Al2O3 support, and denotes this as B.
[0021] 2.0242 g of niobium oxalate hydrate was dissolved in deionized water and labeled as solution C. 0.0930 g of diammonium hydrogen phosphate was added to solution C and labeled as solution D. Support B was dispersed in solution D and stirred continuously for 6 hours using magnetic stirring. The solution was then dried at 120°C for 12 hours and finally calcined in a muffle furnace at 500°C in air for 6 hours. The resulting catalyst contained 5 wt% of the active component Nb and 0.5 wt% of the auxiliary component P (both are oxides relative to the support content), denoted as NP / TA.
[0022] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 340℃, the pressure was 0.20 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 17.90% and a methyl methacrylate selectivity of 86.60%.
[0023] Example 2
[0024] 1.75g of neutral silica sol (silicon content 40%) was dissolved in 15g of deionized water, denoted as solution A; 10g of carrier γ-Al2O3 was weighed and added to solution A, and stirred continuously at 25℃ for 10h under magnetic stirring; then dried at 120℃ for 12h, and the dried solid was calcined at 450℃ in air atmosphere for 4h. The product obtained is 7wt% Si modified γ-Al2O3 carrier, denoted as B.
[0025] 3.4195 g of niobium ammonium oxalate was dissolved in deionized water and denoted as solution C. 0.1394 g of ammonium dihydrogen phosphate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 6 h using magnetic stirring. The solution was then dried at 120 °C for 12 h and finally calcined in a muffle furnace at 500 °C in air atmosphere for 6 h. The resulting catalyst had an active component Nb content of 15 wt% and an auxiliary component P content of 0.86 wt% (both are oxides relative to the support content), denoted as NP / SiA.
[0026] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1.5, the reaction temperature was 340℃, the pressure was 0.05 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 27.40% and a methyl methacrylate selectivity of 89.70%.
[0027] Example 3
[0028] 0.94 g of zirconium oxynitrate was dissolved in 15 g of deionized water and labeled as solution A. Then, 10 g of γ-Al₂O₃ support was dispersed in solution A and stirred continuously at 80 °C for 4 h under magnetic stirring. The solution was then dried at 120 °C for 6 h. After drying, the solid was calcined at 400 °C in air for 3 h. The resulting product was the 5 wt% Zr-modified γ-Al₂O₃ support and labeled as B.
[0029] 1.9930 g of basic magnesium carbonate was dissolved in deionized water and labeled as solution C. 0.2630 g of ammonium phosphate was added to solution C and labeled as solution D. Support B was dispersed in solution D and stirred continuously for 2 hours using a magnetic stirrer. The solution was then dried at 120°C for 4 hours and finally calcined in a muffle furnace at 550°C in air for 6 hours. The resulting catalyst contained 10 wt% Mg (active component) and 1.5 wt% P (both are oxides relative to the support content), denoted as MP / ZrA.
[0030] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 20.20% and a methyl methacrylate selectivity of 76.10%.
[0031] Example 4
[0032] 1.19 g of titanium tetrachloride was dissolved in 15 ml of deionized water, and this solution was denoted as solution A. 10 g of the support γ-Al₂O₃ was weighed and added to solution A. The mixture was stirred at 100 °C for 2 h under magnetic stirring. Then it was dried at 120 °C for 12 h. After drying, the solid was calcined at 550 °C in air for 4 h. The product obtained was the 5 wt% Ti-modified γ-Al₂O₃ support, denoted as B.
[0033] 2.9081 g of magnesium citrate was dissolved in deionized water and labeled as solution C. 0.4398 g of silver nitrate was added to solution C and labeled as solution D. Support B was dispersed in solution D and stirred continuously for 6 hours using magnetic stirring. The solution was then dried at 120°C for 12 hours and finally calcined in a muffle furnace at 300°C in air for 10 hours. The resulting catalyst contained 10 wt% of the active component Mg and 3 wt% of the auxiliary agent Ag (both are oxides relative to the support content), and was labeled as MA / TA.
[0034] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 360℃, the pressure was 0.10 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 18.40% and a methyl methacrylate selectivity of 86.10%.
[0035] Example 5
[0036] 2.50g of neutral silica sol (silicon content 40%) was dissolved in 15g of deionized water, denoted as solution A; 10g of carrier γ-Al2O3 was added to solution A and stirred continuously at 25℃ for 16h under magnetic stirring; then dried at 120℃ for 12h, and the dried solid was calcined at 400℃ in air for 6h. The product obtained was 10wt% Si-modified γ-Al2O3 carrier, denoted as B.
[0037] 10.6416 g of magnesium acetate was dissolved in deionized water and labeled as solution C. 0.0357 g of silver carbonate was added to solution C and labeled as solution D. Support B was dispersed in solution D and stirred magnetically for 2 hours. The solution was then dried at 120°C for 10 hours and finally calcined in a muffle furnace at 500°C in air for 6 hours. The resulting catalyst contained 20 wt% Mg (active component) and 0.3 wt% Ag (auxiliary component) (both are oxides relative to the support content), denoted as MA / SiA.
[0038] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:2, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 1.5 h⁻¹. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 16.80% and a methyl methacrylate selectivity of 74.10%.
[0039] Example 6
[0040] 0.38 g of zirconium oxynitrate was dissolved in 15 g of deionized water and denoted as solution A. Then, 10 g of γ-Al₂O₃ support was dispersed in solution A and stirred continuously at 50 °C for 6 h under magnetic stirring. Then, it was dried at 120 °C for 5 h. After drying, the solid was calcined at 400 °C in air for 6 h. The product obtained was the 2 wt% Zr-modified γ-Al₂O₃ support and denoted as B.
[0041] 6.8113 g of cesium acetate was dissolved in deionized water and denoted as solution C; 0.0032 g of ammonium metavanadate was added to solution C and denoted as solution D; support B was dispersed in solution D and stirred continuously for 2 h with magnetic stirring; then dried at 100 °C for 12 h, and finally calcined in a muffle furnace at 450 °C in air atmosphere for 5 h. The obtained catalyst had an active component Cs content of 50 wt% and an auxiliary agent V content of 0.05 wt% (both are the content of oxides in the support), denoted as CV / ZrA;
[0042] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 360℃, the pressure was 0.15 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 29.10% and a methyl methacrylate selectivity of 90.60%.
[0043] Example 7
[0044] 2.37 g of titanium tetrachloride was dissolved in 15 ml of deionized water, and this solution was denoted as solution A. 10 g of the support γ-Al2O3 was weighed and added to solution A. The mixture was stirred at 90 °C for 2 h under magnetic stirring. Then it was dried at 120 °C for 6 h. After drying, the solid was calcined at 550 °C in air for 4 h. The product obtained was the 10 wt% Ti-modified γ-Al2O3 support, denoted as B.
[0045] 0.6037 g of cesium carbonate was dissolved in deionized water and denoted as solution C. 0.7590 g of ferric nitrate nonahydrate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 6 hours using a magnetic stirrer. The solution was then dried at 100°C for 12 hours and finally calcined in a muffle furnace at 500°C in air for 6 hours. The resulting catalyst contained 6 wt% of active component Cs and 2.5 wt% of auxiliary agent Fe (both are oxides relative to the support content), denoted as CF / TA.
[0046] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 340℃, the pressure was 0.20 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 23.50% and a methyl methacrylate selectivity of 87.40%.
[0047] Example 8
[0048] 6.25g of neutral silica sol (silicon content 40%) was dissolved in 15g of deionized water, denoted as solution A; 10g of γ-Al2O3 support was weighed and added to solution A, and stirred continuously at 25℃ for 24h under magnetic stirring; then dried at 120℃ for 12h, and the dried solid was calcined at 450℃ in air atmosphere for 4h. The product obtained is the 25wt% Si-modified γ-Al2O3 support, denoted as B.
[0049] 0.1284 g of cesium sulfate was dissolved in deionized water and denoted as solution C. 0.1647 g of ferric citrate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 6 hours using magnetic stirring. The solution was then dried at 120°C for 4 hours and finally calcined in an air atmosphere at 800°C in a muffle furnace for 3 hours. The resulting catalyst contained 1 wt% of active component Cs and 5 wt% of auxiliary agent Fe (both are oxides relative to the support content), denoted as CF / SiA.
[0050] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1.5, the reaction temperature was 340℃, the pressure was 0.05 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 20.50% and a methyl methacrylate selectivity of 85.40%.
[0051] Example 9
[0052] 1.50 g of zirconium oxynitrate was dissolved in 15 g of deionized water and labeled as solution A. Then, 10 g of γ-Al₂O₃ support was dispersed in solution A and stirred continuously at 80 °C for 4 h under magnetic stirring. The solution was then dried at 120 °C for 6 h. After drying, the solid was calcined at 400 °C in air for 3 h. The resulting product was the 8 wt% Zr-modified γ-Al₂O₃ support and labeled as B.
[0053] 2.0749 g of cesium nitrate was dissolved in deionized water and denoted as solution C. 0.2710 g of basic copper carbonate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 2 hours using a magnetic stirrer. The solution was then dried at 120°C for 6 hours and finally calcined in a muffle furnace at 550°C in air for 6 hours. The resulting catalyst contained 15 wt% of active component Cs and 1.3 wt% of auxiliary component Cu (both are oxides relative to the support content), denoted as CC / ZrA.
[0054] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 18.90% and a methyl methacrylate selectivity of 80.60%.
[0055] Example 10
[0056] 0.47 g of titanium tetrachloride was dissolved in 15 ml of deionized water, and this solution was denoted as solution A. 10 g of the support γ-Al2O3 was weighed and added to solution A. The mixture was stirred at 40 °C for 2 h under magnetic stirring. Then it was dried at 120 °C for 5 h. After drying, the solid was calcined at 550 °C in air for 4 h. The product obtained was the 2 wt% Ti-modified γ-Al2O3 support, denoted as B.
[0057] 1.4586 g of potassium citrate was dissolved in deionized water and labeled as solution C. 0.3467 g of copper citrate was added to solution C and labeled as solution D. Support B was dispersed in solution D and stirred magnetically for 6 hours. The solution was then dried at 120°C for 12 hours and finally calcined in a muffle furnace at 500°C in air for 6 hours. The resulting catalyst contained 7 wt% of active component K and 2.5 wt% of auxiliary component Cu (both are oxides relative to the support content), denoted as KC / TA.
[0058] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 360℃, the pressure was 0.10 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 26.40% and a methyl methacrylate selectivity of 87.90%.
[0059] Example 11
[0060] 1.25g of neutral silica sol (silicon content 40%) was dissolved in 15g of deionized water, denoted as solution A; 10g of carrier γ-Al2O3 was added to solution A and stirred continuously at 60℃ for 8h under magnetic stirring; then dried at 120℃ for 12h, and the dried solid was calcined at 400℃ in air for 6h. The product obtained was 5wt% Si-modified γ-Al2O3 carrier, denoted as B.
[0061] 0.8672 g of potassium hydrogen phthalate was dissolved in deionized water and denoted as solution C. 0.2126 g of copper nitrate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 2 hours using magnetic stirring. The solution was then dried at 120°C for 10 hours and finally calcined in a muffle furnace at 600°C in air for 4 hours. The resulting catalyst contained 2 wt% of active component K and 3.5 wt% of auxiliary component Cu (both are oxides relative to the support content), denoted as KC / SiA.
[0062] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:2, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 1.5 h⁻¹. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 21.20% and a methyl methacrylate selectivity of 79.10%.
[0063] Example 12
[0064] Weigh 2.00g of diatomaceous earth and 10g of γ-Al2O3 carrier, stir and mix them, and then ball mill them at 200rpm for 2h. Then dry them at 100℃ for 1h, and calcine the dried solid at 400℃ in air atmosphere for 6h. The product obtained is 20wt% γ-Al2O3 carrier modified with diatomaceous earth, denoted as B.
[0065] 1.7341 g of potassium citrate was dissolved in deionized water and denoted as solution C. 0.3101 g of copper nitrate trihydrate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 2 h with magnetic stirring. Then it was dried at 100 °C for 12 h and finally calcined in a muffle furnace at 500 °C in air atmosphere for 6 h. The resulting catalyst had an active component K content of 8 wt% and an auxiliary agent Cu content of 1.5 wt% (both are oxides in the proportion of the support), denoted as KC / SA.
[0066] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 360℃, the pressure was 0.15 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 20.40% and a methyl methacrylate selectivity of 80.10%.
[0067] Example 13
[0068] Weigh out 3g of kaolin and 10g of γ-Al2O3 carrier, mix them and add them to 50ml of ethylene glycol solution, which is denoted as solution A. Stir continuously at 30℃ for 3h under magnetic stirring. Dry at 120℃ for 12h. After drying, calcine the solid at 400℃ in air atmosphere for 6h. The product obtained is 30wt% γ-Al2O3 carrier modified with diatomaceous earth, which is denoted as B.
[0069] 0.4405 g of anhydrous potassium carbonate was dissolved in deionized water and denoted as solution C; 0.3539 g of copper acetate was added to solution C and denoted as solution D; support B was dispersed in solution D and stirred continuously for 2 h with magnetic stirring; then dried at 120 °C for 2 h, and finally calcined in a muffle furnace at 500 °C in air atmosphere for 6 h. The resulting catalyst had an active component K content of 3 wt% and an auxiliary agent Cu content of 4.7 wt% (both are oxides in the proportion of the support), denoted as KC / GA;
[0070] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 340℃, the pressure was 0.15 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 17.30% and a methyl methacrylate selectivity of 79.90%.
[0071] Example 14
[0072] 3.75g of neutral silica sol (silicon content 40%) was dissolved in 15g of deionized water, denoted as solution A; 10g of carrier γ-Al2O3 was weighed and added to solution A, and stirred continuously at 25℃ for 2h under magnetic stirring; then dried at 120℃ for 12h, and the dried solid was calcined at 450℃ in air atmosphere for 4h. The product obtained is 15wt% Si modified γ-Al2O3 carrier, denoted as B.
[0073] 3.1885 g of potassium bicarbonate was dissolved in deionized water and denoted as solution C; 0.3590 g of lanthanum nitrate was added to solution C and denoted as solution D; support B was dispersed in solution D and stirred continuously for 6 h with magnetic stirring; then dried at 120 °C for 12 h, and finally calcined in a muffle furnace at 650 °C in air atmosphere for 4 h. The resulting catalyst had an active component K content of 15 wt% and an auxiliary component La content of 1.2 wt% (both are oxides in the proportion of the support), denoted as KL / SiA;
[0074] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1.5, the reaction temperature was 340℃, the pressure was 0.05 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 23.10% and a methyl methacrylate selectivity of 75.60%.
[0075] Example 15
[0076] 2.81 g of zirconium oxynitrate was dissolved in 15 g of deionized water and labeled as solution A. Then, 10 g of γ-Al₂O₃ support was dispersed in solution A and stirred continuously at 80 °C for 4 h under magnetic stirring. The solution was then dried at 120 °C for 6 h. After drying, the solid was calcined at 400 °C in air for 3 h. The resulting product was the 15 wt% Zr-modified γ-Al₂O₃ support and labeled as B.
[0077] 1.0732 g of potassium nitrate was dissolved in deionized water and denoted as solution C. 0.3190 g of lanthanum nitrate hexahydrate was added to solution C and denoted as solution D. Support B was dispersed in solution D and stirred continuously for 2 hours using magnetic stirring. The solution was then dried at 120 °C for 4 hours and finally calcined in a muffle furnace at 550 °C in air atmosphere for 4 hours. The resulting catalyst contained 5 wt% of active component K and 2.4 wt% of auxiliary component La (both are oxides relative to the support content), denoted as KL / ZrA.
[0078] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 20.60% and a methyl methacrylate selectivity of 87.40%.
[0079] Comparative Example 1
[0080] 2.0242 g of niobium oxalate hydrate was dissolved in deionized water and denoted as solution A. 0.0930 g of diammonium hydrogen phosphate was added to solution A and denoted as solution B. 10 g of γ-Al₂O₃ support was added to solution B and stirred continuously at 60 °C for 2 h under magnetic stirring. The solution was then dried at 120 °C for 12 h and finally calcined in a muffle furnace at 500 °C in air atmosphere for 6 h. The resulting catalyst contained 5 wt% of active component Nb and 0.5 wt% of support P (both are oxides relative to the support content), denoted as NP / A.
[0081] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 340℃, the pressure was 0.20 MPa, and the LHSV was 3 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 13.50% and a methyl methacrylate selectivity of 80.60%.
[0082] Comparative Example 2
[0083] 2.0749 g of cesium nitrate was dissolved in deionized water and labeled as solution A. 0.2710 g of basic copper carbonate was added to solution A and labeled as solution B. 10 g of γ-Al₂O₃ support was added to solution B and stirred continuously at 80 °C for 4 h under magnetic stirring. The solution was then dried at 120 °C for 6 h and finally calcined in a muffle furnace at 550 °C in air for 6 h. The resulting catalyst contained 15 wt% of active component Cs and 1.3 wt% of support Cu (both are oxides relative to the support content), denoted as CC / A.
[0084] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:1, the reaction temperature was 360℃, the pressure was 0.05 MPa, and the LHSV was 2 h. -1 The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methyl propionate conversion rate of 20.10% and a methyl methacrylate selectivity of 70.10%.
[0085] Comparative Example 3
[0086] 0.4405 g of anhydrous potassium carbonate was dissolved in deionized water and labeled as solution A; 0.3539 g of copper acetate was added to solution A and labeled as solution B; 10 g of kaolin support was added to solution B and stirred continuously for 3 h with magnetic stirring; then dried at 120 °C for 2 h, and finally calcined in a muffle furnace at 500 °C in air atmosphere for 6 h. The resulting catalyst had an active component K content of 3 wt% and an auxiliary agent Cu content of 4.7 wt% (both are oxides in the carrier content), labeled as KC / G;
[0087] The obtained sample was pressed into tablets to 40-60 mesh and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The molar ratio of methyl propionate to formaldehyde was 1:3, the reaction temperature was 340℃, the pressure was 0.15 MPa, and the LHSV was 3 h. -1The carrier gas was an oxygen-containing inert atmosphere, with N2 as the inert gas. Online gas chromatography was used for monitoring; final analysis showed that the methyl propionate conversion rate was higher than 16.50%, and the methyl methacrylate selectivity was higher than 70.30%.
[0088] Comparisons between Comparative Example 1 and Example 1, Comparative Example 2 and Example 9, and Comparative Example 3 and Example 13 revealed that, under the same active components, additives, and evaluation conditions, the catalysts without modified supports exhibited inferior catalytic performance compared to the modified catalysts, and their lifespans were also shorter. This may be because the modification of the support forms a stable Al-OM structure, which makes the catalyst structure more stable. Furthermore, the modification provides the support with more weakly acidic and moderately acidic sites. Simultaneously, the loading of basic active components gives the catalyst certain basic sites, thus constructing suitable acid-base sites, resulting in higher activity and stability.
[0089] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A method for preparing a metal-modified Al₂O₃ aldol condensation catalyst, characterized in that: Al2O3 was modified by a modifying agent M, which was one or more of the precursor solutions of Si, Zr, and Ti, or one or more of diatomaceous earth or kaolin. The active component X is one or more precursor salts of metals Nb, Mg, Cs, and K, and its content relative to the support is 50 wt% based on metal oxides; the auxiliary agent Z is a precursor salt of metal V, and its content relative to the support is 0.05 wt% based on metal oxides; the precursor salt of the auxiliary agent Z is ammonium metavanadate. The active component X and the auxiliary agent Z are loaded onto the modified support M-Al2O3 using an impregnation method; in the catalyst, the modifying agent M accounts for 1-30 wt% relative to the Al2O3 support. The modification treatment of the catalyst support Al2O3 is as follows: the support Al2O3 is added to one or more solutions of silica sol, zirconium oxynitrate, zirconium nitrate, tetrabutyl titanate, n-propyl titanate, and tetraethyl titanate, and stirred at 25-100 °C for 2-24 h, and then the water is evaporated and dried; or the support Al2O3 is mechanically mixed with one or more of diatomaceous earth and kaolin.
2. The catalyst preparation method according to claim 1, characterized in that: The active component X includes one or more of the following: carbonate, acetate, and citrate of metallic Mg; oxalate of Nb; acetate, carbonate, sulfate, and nitrate of Cs; and citrate, carbonate, bicarbonate, and nitrate of K.
3. The catalyst preparation method according to claim 1, characterized in that: The contents of active component X and auxiliary agent Z relative to the modified carrier are 50 wt% and 0.05 wt%, respectively, both calculated as metal oxides.
4. The catalyst preparation method according to any one of claims 1-3, characterized in that: In the catalyst, the modified support M-Al2O3 is added to a mixed solution of the active component precursor salt and the auxiliary agent precursor salt, mixed thoroughly and dried, and then calcined in air at 300-800 °C for 3-10 h to obtain the catalyst.
5. A catalyst prepared by any one of the preparation methods described in claims 1-4.
6. The use of the catalyst according to claim 5 in the aldol condensation reaction process.
7. The application of the catalyst according to claim 6, characterized in that: Using a fixed-bed reactor, the catalyst is filled in the middle section of the bed. The catalyst is a 20-60 mesh shaped catalyst, and the upper and lower sections of the bed are filled with quartz sand, respectively. The raw materials are a mixed solution of formaldehyde and methyl propionate or an aqueous mixed solution of formaldehyde and methyl propionate; wherein the carrier gas is N2, and the molar ratio of methyl propionate to formaldehyde is 1:(1-3); the reaction is carried out at 200-450 ℃ under normal pressure, with an LHSV of 0.1-3 h. -1 The product is a mixed solution containing methyl methacrylate and methacrylic acid.
Citation Information
Patent Citations
Zr-Cs series methyl methacrylate catalyst added with modification auxiliary agent and preparation method thereof
CN102350336A
A method for preparing methyl methacrylate from methyl propionate and formaldehyde
CN102775302B
Method for producing methyl methacrylate by methyl acetate and formaldehyde
CN104513163A
Polymer modified supported metal catalyst and preparation method and application thereof
CN109225192A
Process for refining methacrylic acid
EP0710643A1