An aerosol for forming a dense protective layer on the surface of metal parts

By applying an aerosol containing hexaphosphate metaphosphate, polyvinylidene fluoride emulsion and other ingredients on the surface of metal parts, a dense protective film is formed, which solves the problem of failure of metal parts due to corrosion and wear, and significantly improves the corrosion resistance and Protective capabilities extend service life.

CN118109807BActive Publication Date: 2024-10-18ZHEJIANG LUDAO TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410247840.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2024-10-18
Estimated Expiration
2044-03-05

AI Technical Summary

Technical Problem

Metal parts often fail due to corrosion and wear during use. Existing technologies are difficult to effectively improve their corrosion resistance and protection capabilities, resulting in shortened service life and safety risks.

Method used

Using an aerosol including hexaphosphate metaphosphate, polyvinylidene fluoride emulsion, titanium sulfate, nanocomposite particles, nitric acid, sodium zirconate and sodium silicate, through the embedding of nanocomposite particles and the emulsion of polyvinylidene fluoride Synergistically, they form a dense protective film and improve the corrosion resistance and adhesion strength of metal parts.

Benefits of technology

It significantly improves the corrosion resistance of metal parts and the density of the protective film, extends the service life of the protective film, reduces friction and wear, and significantly improves the overall protective effect of metal parts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an aerosol for forming a dense protective layer on the surface of a metal part, relates to the technical field of metal treatment, and comprises the following components by weight: hexaphosphoric acid salt, polyvinylidene fluoride emulsion, titanium sulfate, sulfuric acid, nano-composite particles, nitric acid, sodium zirconate, sodium silicate, and deionized water; the invention provides an aerosol for forming a dense protective layer on the surface of a metal part, which can form a uniform and dense protective film with high gloss and good corrosion resistance on the surface of the metal part. Through the formation of the protective film, the protective effect on the metal part can be greatly improved, thereby not only effectively reducing the friction and wear of the metal part, but also greatly improving the corrosion resistance of the metal part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal treatment, in particular to an aerosol for forming a dense protective layer on the surface of a metal part. Background Art

[0002] Metal parts are generally made of various metals. Commonly used metals include iron, copper, aluminum, etc., which are widely used.

[0003] The failure modes of most metal parts are generally the following: elastic or plastic deformation, wear, fracture and corrosion.

[0004] In most working environments, over 60% of failures are caused by corrosion and wear after long-term use, especially for iron and metal parts. Failures due to corrosion account for over 30% of the total failures each year. The corrosion of metal parts will not only cause a significant reduction in the mechanical properties of the metal parts, shortening their service life, but will also affect the safe operation of the entire equipment.

[0005] Therefore, it is necessary to perform specific protective treatment on the surface of metal parts to improve the surface protection ability of metal parts, thereby increasing the service life of metal parts and reducing the occurrence of corrosion of metal parts.

[0006] Based on this, an aerosol is provided for forming a dense protective layer on the surface of metal parts to process metals in post-processing plants and improve resource utilization. Summary of the invention

[0007] The purpose of the present invention is to provide an aerosol for forming a dense protective layer on the surface of a metal part, so as to solve the shortcomings of the prior art.

[0008] The technical solution adopted by the present invention is as follows:

[0009] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following ingredients by weight: 2-5 parts of hexaphosphoric acid salt, 18-22 parts of polyvinylidene fluoride emulsion, 1-1.5 parts of titanium sulfate, 5-10 parts of sulfuric acid, 3-3.5 parts of nanocomposite particles, 2-3 parts of nitric acid, 1-3 parts of sodium zirconate, 0.1-0.3 parts of sodium silicate, and 100-110 parts of deionized water;

[0010] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0011] As a further technical solution: the method for preparing the nanocomposite particles is:

[0012] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 80-85° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0013] The pH was adjusted using sulfuric acid solution;

[0014] Among them, the mass fraction of sulfuric acid solution is 20%;

[0015] Among them, the speed of heat preservation and stirring is 1000r / min;

[0016] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0017] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0018] Among them, the stirring speed is 2000r / min;

[0019] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0020] Among them, the stirring speed is 500r / min;

[0021] (4) The reaction material obtained in step (3) is washed with anhydrous ethanol for 10 minutes, drained, and then washed again with deionized water for 10 minutes. After vacuum drying, the reaction material is placed in an inert atmosphere for calcination for 30 minutes. After cooling to room temperature, it is ground to obtain nanocomposite particles.

[0022] As a further technical solution: in step (1), the mass ratio of the graphene to the deionized water is 1:10;

[0023] The mass ratio of graphene to potassium permanganate is 1:1.

[0024] As a further technical solution: the mixing ratio of the pretreated graphene particles and the ethanol solution in step (2) is 12-15 g: 100 mL;

[0025] The mass fraction of the ethanol solution is 40%.

[0026] As a further technical solution: the mixing ratio of the graphene ethanol dispersion, cerium nitrate and zirconium nitrate in step (3) is 100mL: 2-3g: 1-1.8g;

[0027] The ammonia water is saturated ammonia water.

[0028] As a further technical solution: in step (4), the vacuum drying is to vacuum dry the reaction material after washing with deionized water at a temperature of 55°C.

[0029] As a further technical solution: in step (4), the inert atmosphere is a nitrogen atmosphere;

[0030] The calcination temperature is 450-460°C;

[0031] The grinding speed is 3500r / min;

[0032] The grinding time is 4 hours.

[0033] As a further technical solution: the hexaphosphoric acid salt is sodium hexaphosphoric acid or potassium hexaphosphoric acid.

[0034] As a further technical solution: the solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0035] Beneficial effects:

[0036] The present invention provides an aerosol for forming a dense protective layer on the surface of a metal part, which can form a uniform and dense protective film with high gloss and good corrosion resistance on the surface of the metal part. Through the formation of the protective film, the protective effect on the metal part can be greatly improved, thereby not only effectively reducing the friction and wear of the metal part, but also greatly improving the corrosion resistance of the metal part.

[0037] The present invention introduces the prepared nanocomposite particles, which can be evenly dispersed in the dense protective film, which not only improves the corrosion resistance of the protective film, but also significantly improves the protective performance and adhesion strength of the formed dense protective film.

[0038] Although directly adding graphene particles can slightly improve the corrosion resistance of the protective film, the presence of graphene particles will affect the surface and cross-sectional morphology of the protective film layer, thereby limiting the further improvement of the corrosion resistance of the protective film. Therefore, the present invention composites the graphene particles to form nano-composite particles, and embeds the nano-composite particles into the internal structure of the protective film layer. The introduced polyvinylidene fluoride emulsion can act as a container for the nano-composite particles, thereby improving the density of the protective film.

[0039] Through the synergistic effect of hexaphosphoric acid salt, titanium sulfate, nano-composite particles, sodium zirconate and sodium silicate, the composition and structure of the protective film can be affected, and the bonding performance between the formed protective film and the surface of the metal part is greatly improved, thereby effectively avoiding the protective film from being unable to continue to protect the metal parts due to the shedding of the protective film, thereby extending the service life of the protective film. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following ingredients by weight: 2 parts of hexaphosphoric acid salt, 18 parts of polyvinylidene fluoride emulsion, 1 part of titanium sulfate, 5 parts of sulfuric acid, 3 parts of nanocomposite particles, 2 parts of nitric acid, 1 part of sodium zirconate, 0.1 part of sodium silicate, and 100 parts of deionized water;

[0043] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0044] The method for preparing nanocomposite particles is as follows:

[0045] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 80° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0046] The pH was adjusted using sulfuric acid solution;

[0047] Among them, the mass fraction of sulfuric acid solution is 20%;

[0048] The speed of the heat preservation stirring is 1000r / min; the mass ratio of graphene to deionized water is 1:10;

[0049] The mass ratio of graphene to potassium permanganate is 1:1.

[0050] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0051] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0052] The stirring speed is 2000 r / min; the mixing ratio of pretreated graphene particles and ethanol solution is 12 g: 100 mL;

[0053] The mass fraction of the ethanol solution is 40%.

[0054] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0055] The stirring speed is 500 r / min; the mixing ratio of graphene ethanol dispersion, cerium nitrate and zirconium nitrate is 100 mL: 2 g: 1 g;

[0056] The ammonia water is saturated ammonia water.

[0057] (4) washing the reaction material obtained in step (3) with anhydrous ethanol for 10 minutes, draining, and then washing the reaction material washed with anhydrous ethanol again with deionized water for 10 minutes, vacuum drying, calcining for 30 minutes in an inert atmosphere, cooling to room temperature, and grinding to obtain nanocomposite particles; vacuum drying is to vacuum dry the reaction material washed with deionized water at a temperature of 55° C.; the inert atmosphere is a nitrogen atmosphere;

[0058] The calcination temperature is 450°C;

[0059] The grinding speed is 3500r / min;

[0060] The grinding time is 4 hours.

[0061] The hexaphosphoric acid salt is potassium hexaphosphoric acid.

[0062] The solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0063] Example 2

[0064] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following ingredients by weight: 3 parts of hexaphosphoric acid salt, 19 parts of polyvinylidene fluoride emulsion, 1.2 parts of titanium sulfate, 6 parts of sulfuric acid, 3 parts of nanocomposite particles, 3 parts of nitric acid, 1.5 parts of sodium zirconate, 0.15 parts of sodium silicate, and 102 parts of deionized water;

[0065] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0066] The method for preparing nanocomposite particles is as follows:

[0067] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 81° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0068] The pH was adjusted using sulfuric acid solution;

[0069] Among them, the mass fraction of sulfuric acid solution is 20%;

[0070] The speed of the heat preservation stirring is 1000r / min; the mass ratio of graphene to deionized water is 1:10;

[0071] The mass ratio of graphene to potassium permanganate is 1:1.

[0072] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0073] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0074] The stirring speed is 2000 r / min; the mixing ratio of pretreated graphene particles and ethanol solution is 13 g: 100 mL;

[0075] The mass fraction of the ethanol solution is 40%.

[0076] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0077] The stirring speed is 500 r / min; the mixing ratio of graphene ethanol dispersion, cerium nitrate and zirconium nitrate is 100 mL: 2.5 g: 1.2 g;

[0078] The ammonia water is saturated ammonia water.

[0079] (4) washing the reaction material obtained in step (3) with anhydrous ethanol for 10 minutes, draining, and then washing the reaction material washed with anhydrous ethanol again with deionized water for 10 minutes, vacuum drying, calcining for 30 minutes in an inert atmosphere, cooling to room temperature, and grinding to obtain nanocomposite particles; vacuum drying is to vacuum dry the reaction material washed with deionized water at a temperature of 55° C.; the inert atmosphere is a nitrogen atmosphere;

[0080] The calcination temperature is 455°C;

[0081] The grinding speed is 3500r / min;

[0082] The grinding time is 4 hours.

[0083] The hexaphosphoric acid salt is sodium hexaphosphoric acid.

[0084] The solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0085] Example 3

[0086] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following ingredients by weight: 4 parts of hexaphosphoric acid salt, 20 parts of polyvinylidene fluoride emulsion, 1.2 parts of titanium sulfate, 8 parts of sulfuric acid, 3.3 parts of nanocomposite particles, 2.5 parts of nitric acid, 2 parts of sodium zirconate, 0.2 parts of sodium silicate, and 105 parts of deionized water;

[0087] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0088] The method for preparing nanocomposite particles is as follows:

[0089] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 82° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0090] The pH was adjusted using sulfuric acid solution;

[0091] Among them, the mass fraction of sulfuric acid solution is 20%;

[0092] The speed of the heat preservation stirring is 1000r / min; the mass ratio of graphene to deionized water is 1:10;

[0093] The mass ratio of graphene to potassium permanganate is 1:1.

[0094] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0095] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0096] The stirring speed is 2000 r / min; the mixing ratio of pretreated graphene particles and ethanol solution is 13 g: 100 mL;

[0097] The mass fraction of the ethanol solution is 40%.

[0098] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0099] The stirring speed is 500 r / min; the mixing ratio of graphene ethanol dispersion, cerium nitrate and zirconium nitrate is 100 mL: 2.5 g: 1.5 g;

[0100] The ammonia water is saturated ammonia water.

[0101] (4) washing the reaction material obtained in step (3) with anhydrous ethanol for 10 minutes, draining, and then washing the reaction material washed with anhydrous ethanol again with deionized water for 10 minutes, vacuum drying, calcining for 30 minutes in an inert atmosphere, cooling to room temperature, and grinding to obtain nanocomposite particles; vacuum drying is to vacuum dry the reaction material washed with deionized water at a temperature of 55° C.; the inert atmosphere is a nitrogen atmosphere;

[0102] The calcination temperature is 458°C;

[0103] The grinding speed is 3500r / min;

[0104] The grinding time is 4 hours.

[0105] The hexaphosphoric acid salt is sodium hexaphosphoric acid.

[0106] The solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0107] Example 4

[0108] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following components by weight: 2 parts of hexaphosphoric acid salt, 22 parts of polyvinylidene fluoride emulsion, 1 part of titanium sulfate, 6 parts of sulfuric acid, 3 parts of nanocomposite particles, 3 parts of nitric acid, 2.5 parts of sodium zirconate, 0.25 parts of sodium silicate, and 105 parts of deionized water;

[0109] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0110] The method for preparing nanocomposite particles is as follows:

[0111] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 85° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0112] The pH was adjusted using sulfuric acid solution;

[0113] Among them, the mass fraction of sulfuric acid solution is 20%;

[0114] The speed of the heat preservation stirring is 1000r / min; the mass ratio of graphene to deionized water is 1:10;

[0115] The mass ratio of graphene to potassium permanganate is 1:1.

[0116] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0117] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0118] The stirring speed is 2000 r / min; the mixing ratio of pretreated graphene particles and ethanol solution is 12 g: 100 mL;

[0119] The mass fraction of the ethanol solution is 40%.

[0120] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0121] The stirring speed is 500 r / min; the mixing ratio of graphene ethanol dispersion, cerium nitrate and zirconium nitrate is 100 mL: 3 g: 1 g;

[0122] The ammonia water is saturated ammonia water.

[0123] (4) washing the reaction material obtained in step (3) with anhydrous ethanol for 10 minutes, draining, and then washing the reaction material washed with anhydrous ethanol again with deionized water for 10 minutes, vacuum drying, calcining for 30 minutes in an inert atmosphere, cooling to room temperature, and grinding to obtain nanocomposite particles; vacuum drying is to vacuum dry the reaction material washed with deionized water at a temperature of 55° C.; the inert atmosphere is a nitrogen atmosphere;

[0124] The calcination temperature is 450°C;

[0125] The grinding speed is 3500r / min;

[0126] The grinding time is 4 hours.

[0127] The hexaphosphoric acid salt is sodium hexaphosphoric acid.

[0128] The solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0129] Example 5

[0130] An aerosol for forming a dense protective layer on the surface of a metal part, comprising the following ingredients by weight: 5 parts of hexaphosphoric acid salt, 22 parts of polyvinylidene fluoride emulsion, 1.5 parts of titanium sulfate, 10 parts of sulfuric acid, 3.5 parts of nanocomposite particles, 3 parts of nitric acid, 3 parts of sodium zirconate, 0.3 parts of sodium silicate, and 110 parts of deionized water;

[0131] The weight ratio of the sodium zirconate to the sodium silicate is 10:1.

[0132] The method for preparing nanocomposite particles is as follows:

[0133] (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 85° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles;

[0134] The pH was adjusted using sulfuric acid solution;

[0135] Among them, the mass fraction of sulfuric acid solution is 20%;

[0136] The speed of the heat preservation stirring is 1000r / min; the mass ratio of graphene to deionized water is 1:10;

[0137] The mass ratio of graphene to potassium permanganate is 1:1.

[0138] (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion;

[0139] The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W;

[0140] The stirring speed is 2000 r / min; the mixing ratio of pretreated graphene particles and ethanol solution is 15 g: 100 mL;

[0141] The mass fraction of the ethanol solution is 40%.

[0142] (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing evenly to obtain a mixed system, then adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material;

[0143] The stirring speed is 500 r / min; the mixing ratio of graphene ethanol dispersion, cerium nitrate and zirconium nitrate is 100 mL: 3 g: 1.8 g;

[0144] The ammonia water is saturated ammonia water.

[0145] (4) washing the reaction material obtained in step (3) with anhydrous ethanol for 10 minutes, draining, and then washing the reaction material washed with anhydrous ethanol again with deionized water for 10 minutes, vacuum drying, calcining for 30 minutes in an inert atmosphere, cooling to room temperature, and grinding to obtain nanocomposite particles; vacuum drying is to vacuum dry the reaction material washed with deionized water at a temperature of 55° C.; the inert atmosphere is a nitrogen atmosphere;

[0146] The calcination temperature is 460°C;

[0147] The grinding speed is 3500r / min;

[0148] The grinding time is 4 hours.

[0149] The hexaphosphoric acid salt is sodium hexaphosphoric acid or potassium hexaphosphoric acid.

[0150] The solid content of the polyvinylidene fluoride emulsion is 40.6%.

[0151] Comparative Example 1:

[0152] The difference from Example 1 is that no nanocomposite particles are added, and the rest of the technical solutions remain unchanged.

[0153] Comparative Example 2:

[0154] The difference from Example 1 is that the nanocomposite particles are replaced with an equal amount of graphene, and the rest of the technical solutions remain unchanged.

[0155] Taking 6030 aluminum alloy as the test object, the aerosols of the embodiment and the comparative example were used for spraying treatment, and the groups were compared:

[0156] The neutral salt spray test was conducted using the neutral salt spray test chamber embodiment and the comparative sample, with the main parameters being: (50±5) g / L sodium chloride solution, pH 6.8, and temperature 35°C:

[0157] Table 1

[0158] Corrosion time / h Example 1 79.4 Example 2 80.5 Example 3 80.2 Example 4 80.0 Example 5 78.1 Comparative Example 1 52.8 Comparative Example 2 55.5 Blank control group 18.4

[0159] The blank control group consisted of 6030 aluminum alloy samples without treatment;

[0160] It can be seen from Table 1 that the surface of the metal part treated with the aerosol prepared by the present invention has better corrosion resistance.

[0161] Further experiments were conducted for 120 hours, and the corrosion areas of the samples in each group were compared:

[0162] Corrosion area = corrosion area / total area

[0163] Table 2

[0164] Corrosion area ratio / % Example 1 26.9 Example 2 25.6 Example 3 26.4 Example 4 27.2 Example 5 28.7 Comparative Example 1 46.7 Comparative Example 2 41.3 Blank control group 72.3

[0165] It can be seen from Table 2 that the corrosion resistance of the metal parts surface treated with the aerosol of the present invention is further improved.

[0166] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. An aerosol for forming a dense protective layer on the surface of metal parts, It is characterized in that The composition comprises the following ingredients by weight: 2-5 parts of hexaphosphoric acid salt, 18-22 parts of polyvinylidene fluoride emulsion, 1-1.5 parts of titanium sulfate, 5-10 parts of sulfuric acid, 3-3.5 parts of nanocomposite particles, 2-3 parts of nitric acid, 1-3 parts of sodium zirconate, 0.1-0.3 parts of sodium silicate, and 100-110 parts of deionized water; The weight ratio of the sodium zirconate to the sodium silicate is 10:1; The method for preparing the nanocomposite particles is as follows: (1) First, graphene is evenly dispersed in deionized water, stirred and mixed, then the pH is adjusted to 3.5, potassium permanganate is added, the temperature is adjusted to 80-85° C., the mixture is stirred and kept warm for 40 minutes, and then filtered and dried to obtain pretreated graphene particles; The pH was adjusted using sulfuric acid solution; Among them, the mass fraction of sulfuric acid solution is 20%; Among them, the speed of heat preservation and stirring is 1000r / min; (2) dispersing the pretreated graphene particles prepared in step (1) into an ethanol solution, and then subjecting the solution to ultrasonic treatment for 1 min, stirring for 5 min, subjecting the solution to ultrasonic treatment for 2 min, stirring for 10 min, and finally subjecting the solution to ultrasonic treatment for 1 min to obtain a graphene ethanol dispersion; The ultrasonic frequency and power of the three ultrasonic treatments were the same, with a frequency of 45 kHz and a power of 550 W; Among them, the stirring speed is 2000r / min; (3) adding cerium nitrate and zirconium nitrate to the graphene ethanol dispersion prepared in step (2), stirring and mixing to obtain a mixed system, adding ammonia water to the mixed system, adjusting the pH of the mixed system to 11 with ammonia water, and continuing to stir for 10 hours in a 60° C. water bath, and filtering to obtain a reaction material; Among them, the stirring speed is 500r / min; (4) The reaction material obtained in step (3) is washed with anhydrous ethanol for 10 minutes, drained, and then washed again with deionized water for 10 minutes. After vacuum drying, the reaction material is placed in an inert atmosphere for calcination for 30 minutes. After cooling to room temperature, it is ground to obtain nanocomposite particles.

2. An aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The mass ratio of the graphene to deionized water in step (1) is 1:10; The mass ratio of graphene to potassium permanganate is 1:

1.

3. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The mixing ratio of the pretreated graphene particles and the ethanol solution in step (2) is 12-15 g: 100 mL; The mass fraction of the ethanol solution is 40%.

4. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The mixing ratio of the graphene ethanol dispersion, cerium nitrate and zirconium nitrate in step (3) is 100 mL: 2-3 g: 1-1.8 g; The ammonia water is saturated ammonia water.

5. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The vacuum drying in step (4) is to vacuum dry the reaction material after washing with deionized water at a temperature of 55°C.

6. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: In step (4), the inert atmosphere is a nitrogen atmosphere; The calcination temperature is 450-460°C; The grinding speed is 3500r / min; The grinding time is 4 hours.

7. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The hexaphosphoric acid salt is sodium hexaphosphoric acid or potassium hexaphosphoric acid.

8. The aerosol for forming a dense protective layer on the surface of a metal part according to claim 1, Features: The solid content of the polyvinylidene fluoride emulsion is 40.6%.

Citation Information

Patent Citations

  • Apparatus and method for aerosol deposition of nanoparticles on a substrate

    CN108026304A

  • Superfine powder paint as well as preparation method and application thereof

    CN108384341A