A method for predicting water damage of asphalt mixture based on material composition and performance

By constructing a prediction model for the water damage resistance of asphalt mixtures, using design parameters and multi-stress creep recovery tests to calculate the peeling inflection point, the problems of high cost and low efficiency in the evaluation of water damage resistance of asphalt mixtures in the existing technology are solved. Efficient material composition selection.

CN118136174BActive Publication Date: 2024-10-18SOUTH CHINA UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410259646.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-07
Publication Date
2024-10-18
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

The existing methods for evaluating the water damage resistance of asphalt mixtures are costly and inefficient, resulting in inefficiencies for engineers and designers in selecting appropriate material compositions.

Method used

Construct a prediction model for the water damage resistance of asphalt mixtures, obtain the design parameters of the asphalt mixture in the prediction model through the functional relationship between the design parameters and the peeling inflection point, conduct a multi-stress creep recovery test and a water-immersed hamburger rutting test, calculate the peeling inflection point, and select the maximum The proportioning scheme of peeling inflection point value.

Benefits of technology

It saves a lot of test costs, improves the efficiency of evaluating the water damage resistance of asphalt mixtures, and optimizes the material composition system that meets the water damage resistance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118136174B_ABST
    Figure CN118136174B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of road engineering technology, and in particular to a method for predicting water damage of asphalt mixtures based on material composition and performance, comprising the following steps: constructing a prediction model for the water damage resistance of asphalt mixtures; testing the crushed surface particle content of selected aggregates, and performing aggregate mix design to determine the aggregate pass rate; determining the amount of asphalt, and performing multiple stress creep recovery tests on the selected asphalt, and calculating the irrecoverable creep compliance under a stress level of 3.2 kPa; inputting the obtained asphalt mixture design parameters into the constructed asphalt mixture water damage resistance prediction model, and calculating the spalling inflection point of the asphalt mixture; comparing the predicted values ​​of different mix design schemes, and selecting the mix design scheme with the maximum spalling inflection point. The present invention adopts the above-mentioned method for predicting water damage of asphalt mixtures based on material composition and performance, which solves the problems of high cost and low efficiency of the asphalt mixture water damage resistance evaluation method in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road engineering, and in particular to a method for estimating water damage of asphalt mixture based on material composition and performance. Background Art

[0002] Water damage is one of the main reasons for early damage to asphalt pavements in my country, which greatly reduces the service life of the pavement and increases the cost of pavement maintenance. In particular, the southern region has a long rainy season and is eroded by rain for a long time, which seriously affects the safety and service life of asphalt pavements. Therefore, it is necessary to evaluate the water damage resistance of asphalt mixtures to help engineers and designers compare the relevant evaluation indicators of asphalt performance and aggregates and select appropriate material composition schemes.

[0003] Common methods for evaluating the water damage resistance of asphalt mixtures disclosed in the prior art include the immersion Marshall test, the immersion splitting strength test, the freeze-thaw splitting strength test, and the immersion rutting test. All of them require the design of asphalt mixture proportions and the preparation of a large number of mixture specimens, consuming a lot of manpower and material resources. In addition, some of the testing equipment is expensive and is not widely used in design and construction units.

[0004] Based on the above problems, there is an urgent need to establish an efficient, simple and low-cost method to predict the water damage resistance of asphalt mixtures and improve the work efficiency of engineers and designers in asphalt performance and aggregate selection. Summary of the invention

[0005] The purpose of the present invention is to provide a method for estimating water damage of asphalt mixture based on material composition and performance, which solves the problems of high cost and low efficiency of the asphalt mixture anti-water damage performance evaluation method in the prior art.

[0006] To achieve the above object, the present invention provides a method for estimating water damage of asphalt mixture based on material composition and performance, comprising the following steps:

[0007] S1 constructs a prediction model for the water damage resistance of asphalt mixtures, which includes the functional relationship between asphalt mixture design parameters and the spalling inflection point;

[0008] S2 performs mixture design on the selected asphalt and aggregate to obtain the asphalt mixture design parameters in the prediction model;

[0009] S2.1 Test the particle content of the crushed surface of the selected aggregate, design the aggregate mix ratio, and determine the aggregate passing rate;

[0010] S2.2 Determine the amount of asphalt, and conduct multiple stress creep recovery tests on the selected asphalt to calculate the irrecoverable creep compliance at a stress level of 3.2 kPa;

[0011] S3 inputs the asphalt mixture design parameters obtained by S2 into the asphalt mixture water damage resistance prediction model constructed by S1 to calculate the spalling inflection point of the asphalt mixture;

[0012] S4 compares the spalling inflection points obtained in S3 and selects the asphalt mixture design scheme with the maximum spalling inflection point value as the asphalt mixture design scheme to be used.

[0013] Preferably, S1, the method for constructing a prediction model for asphalt mixture water damage resistance performance comprises the following steps:

[0014] S1.1 Select asphalt produced in a variety of factories and prepared in the laboratory, use several gradations to design asphalt mixtures, test asphalt mixture design parameters, and count asphalt mixture design parameters that affect the water damage resistance of asphalt mixtures;

[0015] S1.2 The asphalt mixtures designed in S1.1 are rotatably compacted and formed, with a target porosity of 7%. Test specimens are prepared for a water-immersed hamburger rutting test, and a test curve of rutting depth and load action times is obtained to calculate the spalling inflection point;

[0016] S1.3 takes the spalling inflection point of the submerged hamburger rutting test as the dependent variable, and the asphalt mixture design parameters as the independent variables for constructing the model. The stepwise regression control model is used for analysis, and the mixture design parameter variables are introduced one by one. By using the Bayesian information criterion, the mixture design parameter variables that are not significant in the test are deleted, and the optimal model is selected to obtain the best fitting effect.

[0017] Preferably, the asphalt mixture design parameters in S1.1 include asphalt dosage, irrecoverable creep compliance of asphalt at a stress level of 3.2 kPa, aggregate pass rate of key sieve holes, content of coarse aggregate crushing surface particles, angularity of fine aggregate and effective relative density of synthetic mineral aggregate.

[0018] Preferably, the prediction model for the water damage resistance of asphalt mixture constructed by S1 is specifically: y=25883-7199×log(x1)+24276×x2-29120×x3-475485×x4;

[0019] Where, y is the spalling inflection point of the submerged hamburger rutting test;

[0020] x1—irrecoverable creep compliance at 3.2 kPa stress level;

[0021] x2—the ratio of the passing rate of 9.5mm and 4.75mm aggregates, P9.5 / P4.75;

[0022] x3—the content of particles on the crushed surface of coarse aggregate;

[0023] x4—Amount of asphalt used.

[0024] Preferably, S2.1 screens the crushed surface particles of coarse aggregate: if there are two or more particles in the coarse aggregate whose surface projection area is greater than or equal to one quarter of the maximum cross-sectional area and whose surface edges are sharp, calculate the percentage of the mass of the crushed surface particles in the total mass of the coarse aggregate; design the aggregate mix ratio according to engineering experience and specification requirements, and determine the passing rate of 9.5mm and 4.75mm aggregates.

[0025] Preferably, S2.2 subjects the selected asphalt to short-term aging by a rotating thin film heating test, and subjects the asphalt after short-term aging to a multiple stress creep recovery test, wherein the test temperature is consistent with the temperature of a water-immersed hamburger rutting test, and the irrecoverable creep compliance of the asphalt at a stress level of 3.2 kPa is measured.

[0026] Beneficial effects of the present invention:

[0027] Compared with traditional methods, the estimation method of the present invention can predict the spalling inflection point of the asphalt mixture immersion hamburger rutting test by only obtaining the mixture design parameters. The comparison of the water damage resistance of asphalt mixtures with different material compositions can save a lot of test costs, and optimize the material composition system that meets the requirements of the mixture's water damage resistance performance, thereby improving the evaluation efficiency of the asphalt mixture's water damage resistance performance and having certain engineering practical value.

[0028] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a flow chart of a method for estimating water damage of asphalt mixture based on material composition and performance of the present invention;

[0030] Figure 2 It is a gradation curve diagram of three asphalt mixtures of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0032] Example

[0033] Figure 1 is a flow chart of a method for estimating water damage of asphalt mixture based on material composition and performance of the present invention, such as Figure 1As shown, the present invention provides a method for estimating water damage of asphalt mixture based on material composition and performance, comprising the following steps:

[0034] S1 constructs a prediction model for the water damage resistance of asphalt mixtures, which includes the functional relationship between asphalt mixture design parameters and the spalling inflection point;

[0035] The specific method for constructing the prediction model of asphalt mixture anti-water damage performance is as follows:

[0036] S1.1 adopts several gradations for asphalt mixture design. The asphalt used is selected from a variety of factory-produced and laboratory-prepared asphalt. The asphalt mixture design parameters are tested, and the asphalt mixture design parameters that affect the water damage resistance of the asphalt mixture are counted; the asphalt mixture design parameters include asphalt dosage, irreversible creep compliance of asphalt at a stress level of 3.2kPa, aggregate pass rate of key sieve holes, content of coarse aggregate crushing surface particles, angularity of fine aggregate and effective relative density of synthetic mineral aggregate.

[0037] S1.2 The asphalt mixtures designed in S1.1 are rotatably compacted and formed, with a target porosity of 7%. Test specimens are prepared for a water-immersed hamburger rutting test, and a test curve of rutting depth and load action times is obtained to calculate the spalling inflection point;

[0038] S1.3 takes the spalling inflection point of the submerged hamburger rutting test as the dependent variable, and the asphalt mixture design parameters as the independent variables for constructing the model. The stepwise regression control model is used for analysis, and the mixture design parameter variables are introduced one by one. By using the Bayesian information criterion, the mixture design parameter variables that are not significant in the test are deleted, and the optimal model is selected to obtain the best fitting effect.

[0039] The constructed prediction model for the water damage resistance of asphalt mixture is:

[0040] y=25883-7199×log(x1)+24276×x2-29120×x3-475485×x4;

[0041] Where, y is the spalling inflection point of the submerged hamburger rutting test;

[0042] x1—irrecoverable creep compliance at 3.2 kPa stress level;

[0043] x2—the ratio of the passing rate of 9.5mm and 4.75mm aggregates, P9.5 / P4.75;

[0044] x3—the content of particles on the crushed surface of coarse aggregate;

[0045] x4—Amount of asphalt used.

[0046] S2 performs mixture design on the selected asphalt and aggregate to obtain the asphalt mixture design parameters in the prediction model;

[0047] The asphalt used was asphalt from three different sources, with PG grades of PG64-28, PG76-22, and PG58-34, respectively denoted as asphalt I, asphalt II, and asphalt III;

[0048] S2.1 Test the particle content of the crushed surface of the selected aggregate, design the aggregate mix ratio, and determine the aggregate passing rate;

[0049] The performance of the selected aggregates was tested. According to the ASTM D5821 specification, the crushed surface particles of the coarse aggregate were screened. The coarse aggregate contained two or more particles whose surface projection area was greater than or equal to one-fourth of the maximum cross-sectional area and whose surface edges were sharp. The mass of the crushed surface particles was calculated as a percentage of the total mass of the coarse aggregate. The aggregate mix ratio was designed based on engineering experience and specification requirements. The passing rate of 4.75 mm and 9.5 mm aggregates and the amount of asphalt were determined. The three asphalt mixtures were recorded as mixture I, mixture II, and mixture III. The types and design parameters of the three asphalt mixtures are shown in Table 1. The grading curves of the three asphalt mixtures are shown in Table 1. Figure 2 shown.

[0050] Table 1 Three types of asphalt mixtures and design parameters

[0051] serial number Mixture I Mixture Ⅱ Mixture III Mixture type Dense gradation Dense gradation Dense gradation Nominal maximum particle size 19mm 12.5mm 12.5mm Asphalt dosage 5.19% 5.10% 5.30% Content of crushed particles 100.0% 98.0% 98.3% P9.5 / P4.75 1.63 1.45 1.26

[0052] S2.2 Conduct multiple stress creep recovery tests on the selected asphalt and calculate the irrecoverable creep compliance at a stress level of 3.2 kPa;

[0053] According to AASHTO R28, the selected asphalt samples were subjected to a rotating thin film heating test for short-term aging. After short-term aging, the asphalt was prepared using a 25mm parallel plate and 1mm gap setting according to the requirements of AASHTO T315. A multiple stress creep recovery test was conducted, and the irrecoverable creep compliance of the asphalt at a stress level of 3.2kPa was measured at the same test temperature as the immersion hamburger rutting test. The irrecoverable creep compliance of the three asphalts is shown in Table 2.

[0054] Table 2 Irreversible creep compliance of three asphalts

[0055] serial number <![CDATA[Jnr3.2(kPa -1 )]]> <![CDATA[Log(Jnr3.2)(kPa -1 )]]> Asphalt Ⅰ 0.27 -0.572 Asphalt Ⅱ 0.07 -1.155 Asphalt Ⅲ 0.46 -0.337

[0056] S3 inputs the asphalt mixture design parameters obtained by S2 into the asphalt mixture water damage resistance prediction model constructed by S1 to calculate the spalling inflection point of the asphalt mixture;

[0057] In order to verify the accuracy of the model, it is necessary to conduct a water-immersed hamburger rutting test on three asphalt mixtures, namely, I, II, and III, and calculate the spalling inflection points of the three asphalt mixtures. A water-immersed hamburger rutting test was conducted on a rotary compaction specimen with a diameter of D = 150 mm and a height of H = 62 mm at 50°C. The obtained rutting depth-load action number curve was fitted with a sixth-order polynomial function. Tangents were drawn for the creep and spalling stage curves respectively, and the intersection of the two tangents (stripping inflection point) and the number of wheel load actions corresponding to the intersection were obtained. The test results of the spalling inflection points of the three asphalt mixtures were compared with the calculation results of the prediction model and an error analysis was performed. The results are shown in Table 3.

[0058] Table 3 Model error analysis

[0059]

[0060] It can be seen from Table 3 that the water damage prediction model has a good correlation with the results of the submerged hamburger rutting test, so the credibility of the model is verified.

[0061] S4 compares the spalling inflection points obtained in S3, and selects the asphalt mixture design scheme with the maximum spalling inflection point value as the recommended asphalt mixture gradation.

[0062] That is, by comparing the spalling inflection points of mixtures I, II, and III, it can be seen that the predicted value and experimental value of mixture III are both the lowest. The material composition of mixture III does not meet the requirements for the resistance of asphalt mixtures to water damage. It is recommended to use the asphalt and aggregate grading of mixtures I and II.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for estimating water damage of asphalt mixture based on material composition and performance, characterized by: The following steps are involved: S1 builds a prediction model for asphalt mixture anti-water damage performance, which includes the functional relationship between asphalt mixture design parameters and spalling inflection point; The method for constructing a prediction model for the water damage resistance of asphalt mixture includes the following steps: S1.1 Select asphalt produced in a variety of factories and prepared in the laboratory, use several gradations to design asphalt mixtures, test asphalt mixture design parameters, and count asphalt mixture design parameters that affect the water damage resistance of asphalt mixtures; Asphalt mixture design parameters include asphalt dosage, irrecoverable creep compliance of asphalt at 3.2 kPa stress level, aggregate passing rate of key sieve holes, content of coarse aggregate crushing surface particles, angularity of fine aggregate and effective relative density of synthetic mineral aggregate; S1.2 Rotate and compact several asphalt mixtures designed in S1.1 to prepare specimens for water-immersed hamburger rutting tests, obtain the test curve of rutting depth and load action times, and calculate the spalling inflection point; S1.3 The spalling inflection point of the immersion hamburger rutting test was used as the dependent variable, and the asphalt mixture design parameters were used as the independent variables for constructing the model. The stepwise regression control model was used for analysis, and the mixture design parameter variables were introduced one by one. By using the Bayesian information criterion, the mixture design parameter variables that were not significant in the test were deleted, and the optimal model was selected to obtain the best fitting effect. The constructed prediction model of asphalt mixture anti-water damage performance is specifically: y = 25883-7199×log(x1)+24276×x2-29l20×x3-475485×x4; Wherein, y - spalling inflection point of the submerged hamburger rutting test; Irrecoverable creep compliance at stress level x1-3.2kPa; x2-The ratio of the passing rate of 9.5mm and 4.75mm aggregates is P9.5 / P4.75; x3-the content of particles on the crushed surface of coarse aggregate; x4-amount of asphalt; S2 performs mixture design on the selected asphalt and aggregate to obtain the asphalt mixture design parameters in the prediction model; S2.1 Test the particle content of the crushed surface of the selected aggregate, design the aggregate mix ratio, and determine the aggregate passing rate; S2.2 Determine the amount of asphalt, and conduct multiple stress creep recovery tests on the selected asphalt to calculate the irrecoverable creep compliance at a stress level of 3.2 kPa; S3 inputs the asphalt mixture design parameters obtained by S2 into the asphalt mixture water damage resistance prediction model constructed by S1 to calculate the spalling inflection point of the asphalt mixture; S4 compares the spalling inflection points obtained in S3 and selects the asphalt mixture design scheme with the maximum spalling inflection point value as the asphalt mixture design scheme to be used.

2. The method for estimating water damage of asphalt mixture based on material composition and performance according to claim 1 is characterized by: S2.1 Screening of crushed surface particles in coarse aggregate: For particles in coarse aggregate with two or more surfaces whose projected area is greater than or equal to one-fourth of the maximum cross-sectional area and whose surface edges are sharp, calculate the percentage of the mass of the crushed surface particles in the total mass of the coarse aggregate; design the aggregate mix ratio based on engineering experience and specification requirements, and determine the passing rate of 9.5 mm and 4.75 mm aggregates.

3. The method for estimating water damage of asphalt mixture based on material composition and performance according to claim 1 is characterized by: S2.2 The selected asphalt is subjected to short-term aging by a rotating thin film heating test, and the asphalt after short-term aging is subjected to a multiple stress creep recovery test. The test temperature is consistent with the temperature of the water-immersed hamburger rutting test, and the irrecoverable creep compliance of the asphalt at a stress level of 3.2 kPa is measured.

Citation Information

Patent Citations

  • Asphalt mixture virtual performance test prediction method based on mesoscale simulation

    CN106198942A

  • Method for evaluating water damage resistance of asphalt mixture based on molecular dynamics

    CN111161808A

  • Design method for mix proportion of road asphalt mixture in high-temperature environment in desert area

    CN114707320A

  • Asphalt mixture pavement performance evaluation method based on hamburger rut test

    CN114720672A

  • Method for evaluating fusion degree of new asphalt and old asphalt of hot mix plant recycled asphalt mixture

    CN115494224A