A two-dimensional lamellar fuel cell catalyst and preparation method thereof
Through the MXene/two-dimensional high-entropy hydroxide composite catalyst, the problems of slow kinetics of cathode oxygen reduction reaction and insufficient cycle stability in fuel cells are solved, and high-efficiency oxygen reduction reaction and stability are achieved, reducing costs.
Patent Information
- Application Number
- CN202211554696.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-12-06
AI Technical Summary
In fuel cells, the cathode oxygen reduction reaction has slow kinetics, insufficient cycle stability, low anti-toxicity and high cost.
Using MXene/two-dimensional high-entropy hydroxide composite as fuel cell catalyst, two-dimensional sheet layered catalysts are prepared by soaking, washing, drying, ultrasonic mixing and self-assembly, and using the metal conductivity and high-entropy hydrogen of MXene The catalytic activity of oxides achieves high-efficiency oxygen reduction reaction.
It improves the efficiency of oxygen reduction reaction, enhances the cycle stability and reaction kinetics of the battery, provides more reactive sites, and reduces costs.
Smart Images

Figure CN118156522B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells and discloses a two-dimensional lamellar fuel cell catalyst and a preparation method thereof. Background Art
[0002] With the needs of human economic development, fossil energy reserves are decreasing. According to statistics, most fossil energy will be exhausted in this century. At the same time, environmental pollution caused by the burning of fossil fuels and climate change, which are difficult to control and recover, are threatening the global ecosystem. In the long run, the development and use of renewable clean energy to replace fossil energy is the future development direction. Large-scale electrochemical energy storage and conversion devices, such as supercapacitors, secondary electrochemical batteries and fuel cells, can realize the mutual conversion between electrical energy and chemical energy through reversible redox reactions. Among them, fuel cells are valued by people because of their high conversion efficiency and clean and pollution-free.
[0003] Fuel cells convert Gibbs free energy directly into electrical energy through redox reactions, and are not limited by the Carnot cycle of internal combustion engines. The theoretical maximum energy conversion efficiency can reach more than 80%. At the same time, the fuel used by fuel cells is a new type of green renewable energy, and the products produced by the reaction are non-toxic and pollution-free, making fuel cells more environmentally friendly and sustainable.
[0004] However, in the actual application of fuel cells, the reaction kinetics of cathode oxygen reduction is much slower than that of anode oxidation. Oxygen is difficult to adsorb quickly on the electrode surface. At the same time, the activation and dissociation of oxygen-oxygen bonds and the removal of intermediate products are difficult, which leads to slow oxygen reduction reaction kinetics. In addition, there are also defects such as insufficient cycle stability, low anti-poisoning ability and high cost. Therefore, the study of efficient, low-cost and stable cathode oxygen reduction reaction electrocatalysts is one of the research hotspots in this field. Summary of the invention
[0005] In view of the problems existing in the current prior art, the present invention provides a two-dimensional lamellar fuel cell catalyst and a preparation method thereof. The two-dimensional lamellar fuel cell catalyst is mainly composed of a MXene / two-dimensional high entropy hydroxide composite, and the synergistic effect of the two realizes a high-efficiency oxygen reduction reaction and enhances the battery cycle stability.
[0006] The primary purpose of the present invention is to provide a method for preparing a two-dimensional lamellar fuel cell catalyst.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a two-dimensional lamellar fuel cell catalyst comprises the following steps:
[0009] S1. Preparation of two-dimensional MXene sheets: soaking the MAX phase ceramic material in a hydrofluoric acid solution for reaction, heating continuously during the soaking process and changing the solution every 6 hours. After the soaking is completed, washing until the solution is neutral, drying and collecting the product;
[0010] S2. Preparation of two-dimensional high entropy hydroxide: preparing manganese nitrate solution, iron nitrate solution, cobalt nitrate solution, nickel nitrate solution, iridium chloride solution, platinum chloride solution and formamide solution, and dropping the manganese nitrate solution, iron nitrate solution, cobalt nitrate solution, nickel nitrate solution, iridium chloride solution and platinum chloride solution into the formamide solution under stirring, then adding ammonia water to the mixed solution and heating to react at the same time, washing the solution several times until the solution is neutral after the reaction is completed, and drying and collecting the product;
[0011] S3. Preparation of MXene / two-dimensional high entropy hydroxide composite: The MXene prepared in step S1 and the two-dimensional high entropy hydroxide prepared in step S2 are mixed by ultrasound, and then allowed to stand for self-assembly to obtain the MXene / two-dimensional high entropy hydroxide composite.
[0012] Preferably, the MAX phase ceramic material in step S1 includes ternary metal carbides such as Ti3AlC2, Nb3AlC2, and V3AlC2.
[0013] Preferably, in step S1, the mass ratio of the MAX phase ceramic material to the hydrofluoric acid solution is 1:10-20, and the concentration of the hydrofluoric acid solution is 30%-60%.
[0014] Preferably, the soaking time in step S1 is 12 to 48 hours, and the soaking heating temperature is 40° C. to 80° C.
[0015] Preferably, the concentrations of the manganese nitrate solution, iron nitrate solution, cobalt nitrate solution, nickel nitrate solution, iridium chloride solution and platinum chloride solution in step S2 are all 0.1 mol / L to 0.5 mol / L, and the concentration of the formamide solution is 20% to 60%.
[0016] Preferably, in step S2, ammonia water is added until the pH of the mixed solution is 8-10.
[0017] Preferably, the reaction heating temperature in step S2 is 60° C. to 80° C., and the reaction time is 20 minutes to 100 minutes.
[0018] Preferably, in step S3, the mass ratio of the MXene and the two-dimensional high entropy hydroxide is 1 to 5:1, the ultrasonic time is 10 minutes to 30 minutes, and the standing time is 12 hours to 36 hours.
[0019] The present invention also provides a two-dimensional lamellar fuel cell catalyst prepared by the above method.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention provides a fuel cell oxygen reduction reaction catalyst, the main body of which is a MXene / two-dimensional high entropy hydroxide composite. The metallic conductivity of MXene provides a guarantee for the electron transport of the entire reaction, while the metal carbide also exhibits excellent oxygen reduction reaction catalytic effect, improving the overall reaction kinetics. The two-dimensional high entropy hydroxide has a high catalytic activity due to its unique cocktail effect, and can achieve effective oxygen capture and chemical bond catalytic breaking effects. The synergistic effect of the two realizes a highly efficient oxygen reduction reaction.
[0022] 2. The present invention utilizes the self-assembly behavior of two-dimensional materials to organically combine MXene with high entropy hydroxide and form an atomic-level contact interface to achieve charge transfer, further adjust the adsorption energy of the reaction intermediate, and achieve an efficient four-electron oxygen reduction reaction process. At the same time, the two-dimensional sheet stacking structure obtained by self-assembly provides a large number of reactive active sites, which enhances the cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a scanning electron microscope image of the two-dimensional sheet-like MXene / high entropy hydroxide composite catalyst prepared in Example 1 of the present invention.
[0024] Figure 2 This is a chronoamperometric curve of the two-dimensional sheet-like MXene / high entropy hydroxide composite catalyst prepared in Example 1 of the present invention under oxygen conditions in a 0.1 mol / L KOH solution. DETAILED DESCRIPTION
[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Unless otherwise specified, the experimental methods used in the examples of the present invention are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0027] Example 1
[0028] A two-dimensional layered fuel cell catalyst is prepared by the following steps:
[0029] The first step is to prepare two-dimensional MXene sheets
[0030] The commercially purchased MAX phase ceramic material Ti3AlC2 was placed in a 50% hydrofluoric acid solution, with a mass ratio of Ti3AlC2 to the hydrofluoric acid solution of 1:10, and was soaked at 70°C for 24 hours to react and remove aluminum ions. The solution was changed every 6 hours during the soaking process. After the soaking was completed, it was washed with deionized water several times until the solution was neutral, and the product was dried and collected;
[0031] The second step is to prepare two-dimensional high entropy hydroxide
[0032] A 0.1 mol / L manganese nitrate solution, an iron nitrate solution, a cobalt nitrate solution, a nickel nitrate solution, an iridium chloride solution, and a platinum chloride solution are prepared, and a 30% formamide solution is added dropwise into 60 mL of formamide solution under stirring conditions, and then ammonia water is added to the mixed solution until the pH value is 9, and the mixture is heated to 80° C., reacted for 30 minutes, and then washed with deionized water for multiple times until the solution is neutral, and the product is collected by drying;
[0033] Step 3 Preparation of MXene / 2D high entropy hydroxide composite
[0034] The prepared MXene and two-dimensional high entropy hydroxide were mixed in a mass ratio of 2:1 and ultrasonically treated for 20 minutes, and then allowed to stand for 24 hours for self-assembly to obtain a MXene / two-dimensional high entropy hydroxide composite.
[0035] Example 2
[0036] A two-dimensional layered fuel cell catalyst is prepared by the following steps:
[0037] The first step is to prepare two-dimensional MXene sheets
[0038] The commercially purchased MAX phase ceramic material Nb3AlC2 was placed in a 50% hydrofluoric acid solution, with a mass ratio of Nb3AlC2 to the hydrofluoric acid solution of 1:20, and was soaked at 80°C for 12 hours to react and remove aluminum ions. The solution was changed every 6 hours during the soaking process. After the soaking was completed, it was washed with deionized water several times until the solution was neutral, and the product was dried and collected;
[0039] The second step is to prepare two-dimensional high entropy hydroxide
[0040] A 0.5 mol / L manganese nitrate solution, an iron nitrate solution, a cobalt nitrate solution, a nickel nitrate solution, an iridium chloride solution, and a platinum chloride solution are prepared, and a 60% formamide solution is added dropwise into 60 mL of the formamide solution under stirring conditions, and then ammonia water is added to the mixed solution until the pH value is 10, and the mixture is heated to 60° C. After reacting for 60 minutes, the mixture is washed with deionized water for multiple times until the solution is neutral, and the product is collected by drying;
[0041] Step 3 Preparation of MXene / 2D high entropy hydroxide composite
[0042] The prepared MXene and two-dimensional high entropy hydroxide were mixed in a mass ratio of 5:1 and ultrasonically treated for 20 minutes, and then allowed to stand for 36 hours for self-assembly to obtain a MXene / two-dimensional high entropy hydroxide composite.
[0043] Example 3
[0044] A two-dimensional layered fuel cell catalyst is prepared by the following steps:
[0045] The first step is to prepare two-dimensional MXene sheets
[0046] The commercially purchased MAX phase ceramic material V3AlC2 was placed in a 50% hydrofluoric acid solution, with a mass ratio of V3AlC2 to the hydrofluoric acid solution of 1:15, and was soaked at 50°C for 36 hours to react and remove aluminum ions. The solution was changed every 6 hours during the soaking process. After the soaking was completed, it was washed with deionized water several times until the solution was neutral, and the product was dried and collected;
[0047] The second step is to prepare two-dimensional high entropy hydroxide
[0048] A 0.2 mol / L manganese nitrate solution, an iron nitrate solution, a cobalt nitrate solution, a nickel nitrate solution, an iridium chloride solution, and a platinum chloride solution are prepared, and a 50% formamide solution is added dropwise into 60 mL of formamide solution under stirring conditions, and then ammonia water is added to the mixed solution until the pH value is 9, and the mixture is heated to 70° C., reacted for 60 minutes, washed with deionized water for multiple times until the solution is neutral, and dried to collect the product;
[0049] Step 3 Preparation of MXene / 2D high entropy hydroxide composite
[0050] The prepared MXene and two-dimensional high entropy hydroxide were mixed in a mass ratio of 3:1 and ultrasonically treated for 10 minutes, and then allowed to stand for 12 hours for self-assembly to obtain a MXene / two-dimensional high entropy hydroxide composite.
[0051] Experimental example
[0052] The scanning electron microscope image of the two-dimensional sheet-like MXene / high entropy hydroxide composite catalyst prepared in Example 1 of the present invention is as follows: Figure 1 shown.
[0053] The chronoamperometric curve of the two-dimensional sheet-like MXene / high entropy hydroxide composite catalyst prepared in Example 1 of the present invention under oxygen conditions in a 0.1 mol / L KOH solution is as follows: Figure 2 shown.
[0054] Obviously, the specific implementation scheme described above is only a further detailed description of the purpose, technical scheme and beneficial effects of the present invention. It should be understood that the above is only a specific example of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a two-dimensional lamellar fuel cell catalyst, characterized in that: The following steps are involved: S1. Soak the MAX phase ceramic material in a hydrofluoric acid solution, continue heating during the soaking process and replace the solution every 6 hours. After the soaking is completed, wash until the solution is neutral, and dry and collect the product MXene; S2, adding manganese nitrate solution, iron nitrate solution, cobalt nitrate solution, nickel nitrate solution, iridium chloride solution, and platinum chloride solution to the formamide solution, then adding ammonia water to the mixed solution and heating the mixture for reaction, washing the mixture until the solution is neutral after the reaction, and drying and collecting the product two-dimensional high entropy hydroxide; S3, mixing the MXene prepared in step S1 with the two-dimensional high entropy hydroxide prepared in step S2 by ultrasonication, and then standing to self-assemble, to obtain the catalyst; Step S1, the MAX phase ceramic material is Ti3AlC2, Nb3AlC2 or V3AlC2; Step S1, the mass ratio of the MAX phase ceramic material to the hydrofluoric acid solution is 1:10~20, and the concentration of the hydrofluoric acid solution is 30%~60%; Step S2, the concentration of the manganese nitrate solution, iron nitrate solution, cobalt nitrate solution, nickel nitrate solution, iridium chloride solution, platinum chloride solution is 0.1mol / L ~ 0.5mol / L, the concentration of the formamide solution is 20% ~ 60%; In step S3, the mass ratio of MXene to two-dimensional high entropy hydroxide is 1-5:1, the ultrasonic time is 10 minutes to 30 minutes, and the standing time is 12 hours to 36 hours.
2. The method for preparing a two-dimensional lamellar fuel cell catalyst according to claim 1, characterized in that: The soaking time in step S1 is 12 to 48 hours, and the soaking heating temperature is 40° C. to 80° C.
3. The method for preparing a two-dimensional lamellar fuel cell catalyst according to claim 1, characterized in that: In step S2, ammonia water is added until the pH of the mixed solution is 8-10.
4. The method for preparing a two-dimensional lamellar fuel cell catalyst according to claim 1, characterized in that: The reaction heating temperature in step S2 is 60° C. to 80° C., and the reaction time is 20 minutes to 100 minutes.
Citation Information
Patent Citations
Preparation method and application of two-dimensional MXene / iron-cobalt-based composite catalytic material
CN111659431A
Preparation method of platinum-containing high-entropy alloy / MXene composite catalyst
CN113224334A
Platinum-based high-entropy alloy electrocatalyst for oxygen reduction and hydrogen evolution reaction and preparation method of platinum-based high-entropy alloy electrocatalyst
CN115404489A