Preparation method and application of low-temperature electrolyte for lithium metal battery

By physically dehydrating the solvent and additives, a lithium metal battery electrolyte suitable for low-temperature conditions was prepared, which solved the problem of the difficulty of electrolyte freezing and charge transfer of lithium metal batteries at low temperatures, and significantly improved the cycle life and electrochemical performance.

CN118156587BActive Publication Date: 2024-11-26HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410365888.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-11-26
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Lithium metal batteries face problems such as electrolyte freezing, decreasing ion conductance, poor electrode wettability and difficulty in charge transfer under low temperature conditions, resulting in energy density attenuation and short cycle life.

Method used

The solvents and additives were treated by physical dehydration method to prepare a low-temperature electrolyte co-soluble lithium salt with methyl difluoroacetate, hydrofluoroether, perfluorobutylsulfonyl fluoride and fluorovinyl carbonate. The lithium salt was made by magnetic stirring. Fully dissolved to form a lithium metal battery electrolyte suitable for low temperature conditions.

Benefits of technology

It significantly improves the cycle life of lithium metal batteries at low temperatures, with freezing point below -60℃, and the ionic conductivity remains good at -30℃, with wide electrochemical windows, and Coulomb efficiency reaching 90.7%, and shows good performance at low temperatures. Rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118156587B_ABST
    Figure CN118156587B_ABST
Patent Text Reader

Abstract

A preparation method and application of a low-temperature electrolyte for lithium metal batteries, which relates to a preparation method and application of an electrolyte. The present invention provides a method for preparing a low-temperature electrolyte and applying it to a lithium metal battery; the invention obtains a low-temperature electrolyte for a lithium metal battery by dissolving a lithium salt with a solvent and an additive, which significantly improves the cycle life of the lithium metal battery at low temperatures; the electrochemical performance of the low-temperature electrolyte for a lithium metal battery obtained by the present invention is tested, and the freezing experiment results show that the freezing point of the electrolyte is lower than ‑60°C, and the ionic conductivity can be maintained at 0.54mScm at ‑40°C. ‑1 , it can have a wide electrochemical window of 4.88V at -30°C, and the assembled Li||Cu battery can show an average coulombic efficiency of 90.7% at -30°C. The lithium metal battery electrolyte provided by the present invention has good low temperature performance. A low temperature electrolyte for lithium metal batteries is used in lithium metal batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of an electrolyte. Background Art

[0002] Lithium-ion batteries have achieved great success in recent decades. Different climates and harsh application scenarios, such as electric vehicles, polar scientific research, military equipment, and space exploration exposed to ultra-low temperatures, pose increasingly severe challenges to battery operation. At temperatures below -30°C, the interfacial impedance of the battery increases significantly, the capacity decays severely, and huge energy losses occur. Increasing the energy density of the battery system, reducing energy losses, and optimizing interface dynamics can largely solve the anxiety problem under low temperature conditions. Replacing the traditional graphite anode with lithium metal can ensure that the battery energy density exceeds 400Whkg −1 However, the current research on lithium-ion (Li + ) The identification and regulation of kinetic barriers to transport and interfacial reactions at low temperatures are still limited, especially in lithium metal batteries, which hinders the practical feasibility of lithium metal batteries at low temperatures.

[0003] Currently, low-temperature lithium metal batteries face three challenges: (1) the electrolyte becomes more viscous or even freezes at low temperatures, resulting in a decrease in ionic conductivity and poor electrode wettability; (2) charge transfer in the electrode becomes more difficult due to the inherent grain boundary resistance and the slow diffusion of metal ions in the inorganic lattice; (3) the solid electrolyte interlayer (SEI) is more sensitive to Li + The permeability is low. Most of the problems are highly related to the electrolyte. The initial research on low-temperature electrolytes focused on the selection of low-melting-point co-solvents and functional electrolyte additives (such as liquefied gases, carboxylates and difluoroethylene carbonate) to promote ion transport in the electrolyte and in the electrolyte. In recent years, people have begun to pay attention to interfacial reaction kinetic barriers to explain the disadvantages of lithium metal batteries at low temperatures. Under low temperature conditions, the desolvation process is the main interfacial kinetic barrier, and its contribution far exceeds that of other processes. Therefore, the kinetics of the desolvation process can be accelerated by designing a reasonable low-temperature electrolyte by regulating the interaction between the solvent and the solute. Summary of the Invention

[0004] In order to solve the above-mentioned technical problems, the present invention provides a preparation method and application of a low-temperature electrolyte for lithium metal batteries.

[0005] A method for preparing a low-temperature electrolyte for a lithium metal battery is specifically completed by the following steps:

[0006] 1. Physical dehydration:

[0007] adding molecular sieves to the solvent and the additive respectively for physical dehydration to obtain a physically dehydrated solvent and a physically dehydrated additive;

[0008] The solvent in step 1 is one or both of methyl difluoroacetate and hydrofluoroether;

[0009] The additive in step 1 is one or both of perfluorobutylsulfonyl fluoride and fluoroethylene carbonate;

[0010] 2. Evenly mix the physically dehydrated solvent and the physically dehydrated additive, then add lithium salt, and magnetically stir for a period of time until the lithium salt is fully dissolved to obtain a low-temperature electrolyte for lithium metal batteries;

[0011] The lithium salt in step 2 is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide).

[0012] A low-temperature electrolyte for lithium metal batteries is used in lithium metal batteries.

[0013] Advantages of the present invention:

[0014] 1. The present invention provides a method for preparing a low-temperature electrolyte and applying it to lithium metal batteries. The invention obtains a low-temperature electrolyte for lithium metal batteries by co-dissolving a lithium salt with a solvent (one or both of methyl difluoroacetate and hydrofluoroether) and an additive (the additive is one or both of perfluorobutylsulfonyl fluoride and fluoroethylene carbonate), thereby significantly improving the cycle life of lithium metal batteries at low temperatures.

[0015] Second, the electrochemical performance of the low-temperature electrolyte for lithium metal batteries obtained in the present invention was tested. The freezing test results showed that the freezing point of the electrolyte was lower than -60°C, and the ionic conductivity could be maintained at 0.54 mS cm at -40°C. −1 , with a wide electrochemical window of 4.88V at -30°C, and the assembled Li||Cu battery exhibited an average coulombic efficiency of 90.7% at -30°C. When used with an NCM811 cathode, it cycled 200 times at a rate of 0.2C at -30°C, demonstrating the lithium metal battery electrolyte provided by the present invention has excellent low-temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is an image of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 after being kept at -60°C for 1 hour;

[0017] Figure 2 Contact angle test diagrams of the 1M LiTFSI-MPFT low-temperature electrolyte and the 1M LiTFSI-EC / DEC / DMC electrolyte prepared in Example 1;

[0018] Figure 3(a) is the ionic conductivity of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 at temperatures of 60°C to -40°C, (b) is a lithium||stainless steel battery assembled in the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, and the electrochemical stability window of the battery is tested by linear sweep voltammetry (LSV) at a scan rate of 0.2 mV / s in the range of 0-7V; (c) is a lithium||aluminum foil battery assembled in the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, and the electrochemical stability window of the battery is tested by linear sweep voltammetry (LSV) at a scan rate of 0.2 mV / s in the range of 0-7V;

[0019] Figure 4 The average coulombic efficiency diagram of the Li||Cu battery assembled using the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 at room temperature and -30°C is shown in FIG. Figure 4 (a) is room temperature, (b) is -30°C;

[0020] Figure 5 The Li||Li symmetrical battery assembled with the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 was subjected to the low-temperature conditions of -30°C at 0.5, 1, 1.5, and 2 mA cm −2 Rate performance diagram at current density;

[0021] Figure 6 Li||LiCoNiMnO4 assembled using the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1

[0022] (NCM811) Cycling performance curve of full battery at 0.2C rate. DETAILED DESCRIPTION

[0023] Specific embodiment 1: This embodiment is a method for preparing a low-temperature electrolyte for a lithium metal battery, which is specifically completed by the following steps:

[0024] 1. Physical dehydration:

[0025] adding molecular sieves to the solvent and the additive respectively for physical dehydration to obtain a physically dehydrated solvent and a physically dehydrated additive;

[0026] The solvent in step 1 is one or both of methyl difluoroacetate and hydrofluoroether;

[0027] The additive in step 1 is one or both of perfluorobutylsulfonyl fluoride and fluoroethylene carbonate;

[0028] 2. Evenly mix the physically dehydrated solvent and the physically dehydrated additive, then add lithium salt, and magnetically stir for a period of time until the lithium salt is fully dissolved to obtain a low-temperature electrolyte for lithium metal batteries;

[0029] The lithium salt in step 2 is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide).

[0030] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the purity of the solvent in step 1 is 99.99 wt %. The other steps are the same as those in specific embodiment 1.

[0031] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the purity of the additive in step 1 is 99.99 wt %. The other steps are the same as those in specific embodiment 1 or 2.

[0032] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that in step 1, molecular sieves are added to the solvent and additives for physical dehydration to control the moisture content of the solvent and additives to 0 ppm to 20 ppm. The other steps are the same as specific embodiments 1 to 3.

[0033] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the hydrofluoroether in step 1 is 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether. The other steps are the same as those in specific embodiments 1 to 4.

[0034] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the concentration of the lithium salt in the low-temperature electrolyte for lithium metal batteries in step 2 is 0.5 mol / L to 3 mol / L. The other steps are the same as specific embodiments 1 to 5.

[0035] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the volume ratio of the physically dehydrated solvent to the physically dehydrated additive in step 2 is (6-8):(2-4). The other steps are the same as specific embodiments 1 to 6.

[0036] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that the speed of the magnetic stirring in step two is 100 r / min to 400 r / min, and the time of magnetic stirring is 20 min to 40 min.

[0037] Specific embodiments one to seven are the same.

[0038] Specific embodiment 9: This embodiment is an application of a low-temperature electrolyte for lithium metal batteries in lithium metal batteries.

[0039] The following examples are used to verify the beneficial effects of the present invention:

[0040] Example 1: A method for preparing a low-temperature electrolyte for a lithium metal battery is specifically completed by the following steps:

[0041] 1. Physical dehydration:

[0042] adding molecular sieves to the solvent and additive respectively for physical dehydration, controlling the water content of the solvent and additive to 0 ppm, and obtaining a physically dehydrated solvent and a physically dehydrated additive;

[0043] The purity of the solvent described in step 1 is 99.99wt%;

[0044] The purity of the additive described in step 1 is 99.99wt%;

[0045] The solvents described in step 1 are methyl difluoroacetate (MDFA) and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TTE);

[0046] The additives described in step 1 are perfluorobutylsulfonyl fluoride (PBF) and fluoroethylene carbonate (FEC);

[0047] 2. Evenly mix the physically dehydrated solvent and the physically dehydrated additive, then add lithium salt, and stir magnetically for 30 minutes at a speed of 300 r / min until the lithium salt is fully dissolved to obtain a 1M LiTFSI-MPFT low-temperature electrolyte;

[0048] The volume ratio of methyl difluoroacetate (MDFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TTE), perfluorobutylsulfonyl fluoride (PBF) and fluoroethylene carbonate (FEC) in the low-temperature electrolyte for lithium metal batteries described in step 2 is 4:4:1:1;

[0049] The lithium salt described in step 2 is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI);

[0050] The concentration of lithium salt in the low-temperature electrolyte for lithium metal batteries described in step 2 is 1 mol / L.

[0051] Comparative Example: A 1MLiTFSI-EC / DEC / DMC electrolyte was prepared by the following steps: dissolving LiTFSI in a mixed solution of organic solvents including ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC); and magnetically stirring the mixture at 300 rpm for 30 minutes to fully dissolve the lithium salt, thereby obtaining a 1MLiTFSI-EC / DEC / DMC low-temperature electrolyte. The concentration of LiTFSI in the 1MLiTFSI-EC / DEC / DMC low-temperature electrolyte was 1 mol / L; and the organic solvents EC:DMC:DMC were in a ratio of 1:1:1 by volume.

[0052] Figure 1 This is an image of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 after being kept at -60°C for 1 hour;

[0053] from Figure 1 It can be seen that the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 remains in a liquid state at -60°C, indicating that the configured low-temperature electrolyte has a low freezing point and can meet the requirements of testing under extreme environmental conditions.

[0054] The wetting angle test results of the two electrolytes on the NCM811 positive electrode and polypropylene (PP) separator are shown in Figure 2 As shown;

[0055] Figure 2 Contact angle test diagrams of 1M LiTFSI-MPFT low-temperature electrolyte and 1M LiTFSI-EC / DEC / DMC electrolyte prepared in Example 1;

[0056] from Figure 2 It can be seen that the wetting angle of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 on the diaphragm is 9°, while the wetting angle of the 1MLiTFSI-EC / DEC / DMC electrolyte on the diaphragm is 19°, indicating that the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 has good wettability to the positive electrode sheet and the diaphragm, which can ensure good contact between the electrolyte and the positive electrode sheet and the diaphragm, and promote ion transport and electrochemical reaction.

[0057] Figure 3(a) is the ionic conductivity of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 at temperatures of 60°C to -40°C, (b) is a lithium||stainless steel battery assembled in the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, and the electrochemical stability window of the battery is tested by linear sweep voltammetry (LSV) at a scan rate of 0.2 mV / s in the range of 0-7V; (c) is a lithium||aluminum foil battery assembled in the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, and the electrochemical stability window of the battery is tested by linear sweep voltammetry (LSV) at a scan rate of 0.2 mV / s in the range of 0-7V;

[0058] Figure 3 Medium lithium | | stainless steel battery assembly method: the positive electrode is a stainless steel sheet, the negative electrode is a lithium sheet, the separator is a polypropylene separator, and the electrolyte is the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, with a dosage of 70µL. Lithium | | aluminum battery assembly method: the positive electrode is aluminum foil, the negative electrode is a lithium sheet, the separator is a polypropylene separator, and the electrolyte is the 1M LiTFSI prepared in Example 1

[0059] -MPFT low-temperature electrolyte, the dosage is 70µL.

[0060] from Figure 3 (a) It can be seen that the ionic conductivity of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 gradually decreases with decreasing temperature and remains at 0.54 mScm even at -40°C. −1 The electrochemical stability window of stainless steel||lithium battery was tested by linear sweep voltammetry. Figure 3 (b) as shown; Figure 3 (b) The 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 exhibits an oxidation potential of 4.88 V, meeting the requirements for lithium battery cathode materials. When tested on an aluminum electrode, the potential of the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 increased to over 5.8 V, demonstrating that this electrolyte effectively inhibits aluminum corrosion.

[0061] To reveal the compatibility of low-temperature electrolytes with lithium metal anodes, the coulombic efficiency (CE) of Li||Cu batteries was first evaluated.

[0062] Li||Cu battery assembly method: the positive electrode is copper foil, the negative electrode is lithium sheet, the separator is polypropylene separator, and the electrolyte is 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, with a dosage of 70µL.

[0063] Figure 4The average coulombic efficiency diagram of the Li||Cu battery assembled using the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 at room temperature and -30°C is shown in FIG. Figure 4 (a) is room temperature, (b) is -30°C;

[0064] from Figure 4 It can be seen that: using the improved Aurbach method, at room temperature, 1M LiTFSI prepared in Example 1

[0065] The average CE value of the Li||Cu battery assembled with the MPFT low-temperature electrolyte was 97.9%. When the test temperature was further reduced to -30°C, the Li||Cu battery exhibited an average Coulombic efficiency of 90.7%. This demonstrates the superiority of this electrolyte, enabling highly reversible lithium plating / stripping at low temperatures of -30°C.

[0066] Li||Li battery assembly method: the positive and negative electrodes are lithium sheets, the separator is a polypropylene separator, and the electrolyte is the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, with a dosage of 70 μL.

[0067] Figure 5 The Li||Li symmetrical battery assembled with the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 was subjected to the low-temperature conditions of -30°C at 0.5, 1, 1.5, and 2 mA cm −2 Rate performance diagram at current density;

[0068] from Figure 5 It can be seen that the Li||Li symmetrical battery assembled with the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 has a high capacitance at 0.5, 1, 1.5, and 2 mA cm −2 They all have good anti-polarization behavior at current densities of 200 nm and 250 nm, and the interfacial side reactions are slow.

[0069] LiCoNiMnO4 (NCM811) positive electrode sheet: The positive electrode active material is lithium nickel cobalt manganese oxide; the conductive agent is super carbon (Super P); and the binder is polyvinylidene fluoride (PVDF). The weight percentage of positive electrode active material: conductive agent: binder is 96%:2%:2%. Li||LiCoNiMnO4 (NCM811) full cell assembly method: The positive electrode is an NCM811 electrode sheet, the negative electrode is a lithium sheet, the separator is a polypropylene separator, and the electrolyte is the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, used in an amount of 100µL.

[0070] Figure 6 Li||LiCoNiMnO4 assembled using the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1

[0071] (NCM811) Cycling performance curve of full battery at 0.2C rate;

[0072] from Figure 6 It can be seen that the mass loading of the active material NCM811 in the NCM811 electrode is ~10 mg cm −2 . Li||

[0073] The initial discharge specific capacity of the LiCoNiMnO4 (NCM811) full battery is about 110.64 mAh g –1 , after 200 cycles, it dropped to 44.36 mAh g –1 The capacity retention rate is 40%, indicating that the battery assembled using the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 can provide good discharge specific capacity and cycle life at a low temperature of -40°C.

[0074] Commercial NCM811 full battery assembly method: The positive electrode is a commercial NCM811 electrode sheet (active material NCM811 loading ~17.5mgcm ‒2 ), the negative electrode is a lithium sheet, the separator is a polypropylene separator, and the electrolyte is the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1, with a dosage of 100 μL.

[0075] The commercial NCM811 full battery assembled with the 1M LiTFSI-MPFT low-temperature electrolyte prepared in Example 1 has an initial discharge capacity of 145.35 mAh g at 0.1 C at a low temperature of -20 ° C. ‒1 , the initial discharge capacity at 0.1C at low temperature of -30℃ is 120.74mAhg ‒1 , the initial discharge capacity at 0.1C at low temperature of -40℃ is 107.52mAhg ‒1 .

[0076] Example 2: This example differs from Example 1 in that the volume ratio of methyl difluoroacetate (MDFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TTE), perfluorobutylenesulfonyl fluoride (PBF), and fluoroethylene carbonate (FEC) in the low-temperature electrolyte for lithium metal batteries described in Step 2 is 4:6:0:0. That is, perfluorobutylenesulfonyl fluoride (PBF) and fluoroethylene carbonate (FEC) are omitted. All other steps and parameters are the same as in Example 1.

[0077] The commercial NCM811 full battery assembled with the low-temperature electrolyte prepared in Example 2 has an initial discharge capacity of 125 mAh g at 0.1 C at -20 ° C. ‒1 .

[0078] Example 3: This example differs from Example 1 in that the volume ratio of methyl difluoroacetate (MDFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TTE), perfluorobutylenesulfonyl fluoride (PBF), and fluoroethylene carbonate (FEC) in the low-temperature electrolyte for lithium metal batteries described in Step 2 is 4:5:1:0. In other words, fluoroethylene carbonate (FEC) is omitted. All other steps and parameters are the same as in Example 1.

[0079] The commercial NCM811 full battery assembled with the low-temperature electrolyte prepared in Example 3 has an initial discharge capacity of 81.65 mAh g at 0.1 C at -40 ° C. ‒1 .

[0080] Example 4: This example differs from Example 1 in that the volume ratio of methyl difluoroacetate (MDFA), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TTE), perfluorobutylenesulfonyl fluoride (PBF), and fluoroethylene carbonate (FEC) in the low-temperature electrolyte for lithium metal batteries described in Step 2 is 4:5:0:1. That is, perfluorobutylenesulfonyl fluoride (PBF) is omitted. All other steps and parameters are the same as in Example 1.

[0081] The commercial NCM811 full cell was assembled using the low-temperature electrolyte prepared in Example 4. In the resulting low-temperature lithium-ion battery, the initial discharge capacity at 0.1C at a low temperature of -20°C was 120.61 mAh g ‒1 The initial discharge capacity at 0.1C at -30°C is 93.62mAhg ‒1 The initial discharge capacity at 0.1C at -40°C is 74.33mAhg ‒1 .

Claims

1. A method for preparing a low-temperature electrolyte for a lithium metal battery, characterized in that The preparation method is specifically completed according to the following steps:

1. Physical dehydration: Adding molecular sieves to the solvent and the additive respectively for physical dehydration to obtain a physically dehydrated solvent and a physically dehydrated additive; The solvent described in step 1 is methyl difluoroacetate and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether; The additives described in step 1 are perfluorobutylsulfonyl fluoride and fluoroethylene carbonate; 2. Evenly mix the physically dehydrated solvent and the physically dehydrated additive, add lithium salt, and stir magnetically for a period of time until the lithium salt is fully dissolved to obtain a low-temperature electrolyte for lithium metal batteries; The lithium salt described in step 2 is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide); The concentration of lithium salt in the low-temperature electrolyte for lithium metal batteries described in step 2 is 0.5 mol / L to 3 mol / L; The volume ratio of methyl difluoroacetate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, perfluorobutylsulfonyl fluoride and fluoroethylene carbonate in the low-temperature electrolyte for lithium metal batteries described in step 2 is 4:4:1:

1.

2. The method for preparing a low-temperature electrolyte for a lithium metal battery according to claim 1, characterized in that The purity of the solvent in step 1 is 99.99 wt %.

3. The method for preparing a low-temperature electrolyte for a lithium metal battery according to claim 1, characterized in that The purity of the additive in step 1 is 99.99 wt %.

4. The method for preparing a low-temperature electrolyte for a lithium metal battery according to claim 1, characterized in that In step 1, molecular sieves are added to the solvent and the additive respectively for physical dehydration, and the water content in the solvent and the additive is controlled at 0 ppm to 20 ppm.

5. The method for preparing a low-temperature electrolyte for a lithium metal battery according to claim 1, characterized in that The concentration of lithium salt in the low-temperature electrolyte for lithium metal batteries described in step 2 is 0.5 mol / L to 3 mol / L.

6. The method for preparing a low-temperature electrolyte for a lithium metal battery according to claim 1, characterized in that The speed of the magnetic stirring in step 2 is 100 r / min to 400 r / min, and the time of the magnetic stirring is 20 min to 40 min.

7. Use of a low-temperature electrolyte for a lithium metal battery prepared by the preparation method according to claim 1, characterized in that A low-temperature electrolyte for lithium metal batteries is used in lithium metal batteries.