A supported RuM nano alloy catalyst and preparation method thereof
Through ammonia water regulation and strong electrostatic adsorption technology, combined with the atmosphere reduction method, the problem of preparation of RuM nano-alloy catalysts on various carriers has been solved, high dispersion and alloying degree have been improved, and the common problems of RuM catalysts in the existing technology have been solved. suitability and industrial application problems, and improve catalytic activity and selectivity.
Patent Information
- Application Number
- CN202410247048.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-05
AI Technical Summary
It is difficult to efficiently synthesize RuM (M=Cu, Co, Ni, Ag, etc.) bulk phase incompatible nano-alloy catalysts with existing technology, and is greatly affected by the nature of the solvent and the type of carrier, lacks universality, and the reduction of Ru The low potential makes it difficult to generate Ru atoms, and the use of high temperatures and toxic solvents is not conducive to industrial applications.
The pH of the metal precursor solution is adjusted by ammonia water to form an ammonia complex, and the strong electrostatic adsorption theory is used to uniformly adsorb the positively charged metal-ammonia complex on the surface of the carrier, and the supported RuM nanoalloy is prepared by combining the atmosphere reduction method. Catalyst to achieve high dispersion and improved alloying degree.
It has achieved efficient preparation of highly dispersed and highly alloyed RuM nano-alloy catalysts on a variety of carriers, inhibited nanoparticle agglomeration, controlled particle size, improved catalytic activity and selectivity, and is suitable for industrial applications.
Smart Images

Figure CN118162158B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic application, and specifically relates to a supported RuM nano alloy catalyst and a preparation method thereof. Background Art
[0002] Ruthenium (Ru)-based materials are considered as potential substitutes for Pt-based catalysts due to their lower price and similar properties to Pt, but their catalytic activity and selectivity still need to be improved. One of the most effective methods is to introduce a second metal to form an alloy, change the electronic structure and geometric structure of the catalytic active site, and thus improve the catalytic performance. However, Ru thermodynamically prefers to form a hexagonal close-packed (hcp) structure, while most transition metals are face-centered cubic (fcc) structures, which are not easy to form alloys, and Ru 3+ / Ru has a lower reduction potential, which makes it relatively difficult to reduce Ru atoms from the precursor. Reference J.Am.Chem.Soc.2017,139,4643-4646 uses diethylene glycol as solvent and reducing agent, and uses Ru(acac) 3 、Cu(OAc) 2 ·H 2 O as a precursor, RuCu uniform alloy nanoparticles were prepared under vigorous stirring at 220°C. The reaction temperature is relatively high and the organic solvent is a toxic substance. 2 As carrier, RuCl 3 ·3H 2 O、NiCl 2 6H 2 O as a precursor, using TiO 2 Due to the strong interaction between the support and the metal and the hydrogen overflow phenomenon, RuNi alloy catalysts were prepared by the conventional impregnation method, but this method was not effective in the preparation of RuNi alloy catalysts on SiO 2 ,Al 2 O 3 ,ZrO 2 , the ideal RuNi alloy has not been obtained on carriers such as MgO, and lacks certain universality.
[0003] In summary, currently, there are limited methods for efficiently synthesizing bulk-incompatible RuM (M = Cu, Co, Ni, Ag, etc.) nano-alloy catalysts, which are greatly affected by the properties of solvents and the types of carriers. The present invention aims to provide a RuM nano-alloy catalyst with a simple synthesis method, which is applicable to a variety of carriers and has high dispersion and high alloying degree. Summary of the invention
[0004] In order to make up for the shortcomings of the existing technology, 3+ / Ru has a low reduction potential, and it is relatively difficult to reduce Ru atoms from precursors. It is necessary to select suitable precursors to achieve the preparation of Ru alloys. The reaction temperature used in some literature is high, and vigorous stirring is required, which is not conducive to industrial application. The organic solvents used, such as diethylene glycol, are toxic substances and are not environmentally friendly. 2 , Al 2 O 3 , ZrO 2 , it is impossible to obtain an ideal Ru alloy catalyst on a carrier such as MgO, and it lacks a certain universality. The present invention proposes a supported RuM nano-alloy catalyst and a preparation method.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A supported RuM nano alloy catalyst, the supported RuM nano alloy catalyst comprises the following components, in terms of atomic molar percentage, the chemical molecular formula of the supported RuM nano alloy catalyst is Ru x M y / ZT; A RuM alloy structure is formed in the supported RuM nanoalloy catalyst, and the two elements are evenly distributed;
[0007] Where M is the second metal, ZT represents the carrier, Ru x M y is the active component, x / y is the molar ratio of Ru to M, and is in the range of 0.1-10.
[0008] Preferably, M is one of transition metals including Cu, Co, Ni and Ag.
[0009] Preferably, the ZT is SiO 2 、Al 2 O 3 , any one of SBA-15 molecular sieve, ZSM-5 molecular sieve, SUZ-4 molecular sieve, SAPO-34 molecular sieve, and mesoporous carbon.
[0010] Preferably, the Ru x M y The particle size is 2-5 nm.
[0011] Preferably, the molar ratio of Ru to M is 0.1-10.
[0012] Preferably, the Ru loading is 0.1-10%, where the loading is the mass percentage of metal Ru in the carrier.
[0013] A method for preparing a supported RuM nano alloy catalyst comprises the following steps:
[0014] S1. Weigh RuCl 3 Dissolve in deionized water, add 25% ammonia water to the solution to form Ru(OH) 3 Precipitation, continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH 3 ) 6 3+ Exist in the form of complexes;
[0015] S2, weigh the second metal M precursor and dissolve it in deionized water, add ammonia water with a mass concentration of 25% to the solution to form the metal hydroxide precipitate, and continue to add ammonia water until the solid is dissolved to form a transparent solution. At this time, the second metal M precursor is M (NH 3 ) 6 x+ Exist in the form of complexes.
[0016] S3, mixing the solutions obtained in step S1 and step S2, mixing evenly by ultrasonication for 5-10 minutes, continuing to drop ammonia water, adjusting the pH of the solution, regulating the negative charge concentration on the surface of the carrier, and using the mutual attraction of the enriched negative charge on the surface of the carrier to the ammonia complex with positive charge, drop the mixed solution onto the carrier drop by drop, then drying in an oven at 60-100°C for 12-24h, and then drying at 400-800°C and 5-40% H 2 / N 2 atmosphere for 2-6h, with a gas flow rate of 20-80mL / min and an atmosphere furnace heating rate of 2-10℃ / min, to obtain Ru x M y / ZT nano alloy catalyst.
[0017] Preferably, in step S1, RuCl 3 The mass is determined according to the Ru loading amount set for the target catalyst. The Ru loading amount is between 0.1-10%. The volume of deionized water can dissolve the weighed RuCl 3 That’s it, between 1-5ml.
[0018] Preferably, the weighed mass of the second metal in step S2 is determined according to the set molar ratio of Ru to M, within the range of 0.1-10, and the volume of deionized water is sufficient to dissolve the weighed second metal M precursor, which is between 1-5 ml.
[0019] Preferably, in step S3, the solution pH is determined according to the zero charge point pH of the carrier. When the solution pH is greater than the zero charge point, the surface of the carrier is negatively charged.
[0020] The preparation method of the supported RuM catalyst provided above is to adjust the pH of the metal precursor solution by ammonia water, and form an ammonia complex with the metal ions at the same time, and then use the strong electrostatic adsorption theory to make the metal precursor with positive charge be strongly and evenly adsorbed on the surface of the carrier rich in negative charge. After atmospheric reduction, a highly dispersed RuM nano alloy catalyst with a high degree of alloying is finally obtained.
[0021] Compared with the prior art, the technical effects and advantages of the present invention are:
[0022] The supported RuM nano alloy catalyst and preparation method are based on SiO 2 、Al 2 O 3 Using oxides such as RuM as carriers, the pH of the metal precursor solution is adjusted by ammonia water, and at the same time, an ammine complex is formed with the metal ions. Using the theory of strong electrostatic adsorption, the positively charged metal-ammine complex is strongly and evenly adsorbed on the surface of the carrier enriched with negative charges. The catalyst precursor is reduced under a reducing atmosphere to obtain a RuM nanoalloy catalyst.
[0023] The supported RuM nano-alloy catalyst and preparation method thereof, the strong electrostatic adsorption between the precursor and the carrier can effectively inhibit the agglomeration of nano-particles at high temperature, can realize the size control of the RuM nano-particles supported on the carrier, and the uniform distribution of metal elements is conducive to forming a uniform alloy structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is an electron microscope image of the Ru1Co2 / SiO2 catalyst prepared in Example 1 of the present invention;
[0025] Figure 2 The Ru prepared in Example 1 of the present invention 1 Co 2 / SiO 2 Statistical results of catalyst particle size;
[0026] Figure 3 The single metal Ru / SiO 2 Catalyst and Ru prepared in Example 1 1 Co 2 / SiO 2 In-situ infrared spectrum of CO of the catalyst;
[0027] Figure 4 The Ru prepared in Example 2 of the present invention 1 Cu 5 / Al 2 O 3 Electron micrograph of the catalyst;
[0028] Figure 5The Ru prepared in Example 2 of the present invention 1 Cu 5 / Al 2 O 3 Statistical results of catalyst particle size;
[0029] Figure 6 The Ru prepared in Example 3 of the present invention 1 Ni 2 / Al 2 O 3 Electron micrograph of catalyst;
[0030] Figure 7 The Ru prepared in Example 3 of the present invention 1 Ni 2 / Al 2 O 3 Statistical results of catalyst particle size;
[0031] Figure 8 Ru prepared in Example 4 of the present invention 1 Co 5 Electron microscope image of / C catalyst;
[0032] Fig. 9 The Ru prepared in Example 4 of the present invention 1 Co 5 / C catalyst particle size statistics diagram;
[0033] Fig.10 The Ru / SiO 2 Catalyst, Ru in Example 1 1 Co 2 / SiO 2 Catalyst and Ru in Example 2 1 Cu 5 / Al 2 O 3 The curve of propane conversion rate of the catalyst in propane dehydrogenation reaction at 560℃ versus reaction time;
[0034] Fig.11 The Ru / SiO 2 Catalyst, Ru in Example 1 1 Co 2 / SiO 2 Catalyst and Ru in Example 2 1 Cu 5 / Al 2 O 3 The curve of propylene selectivity changing with time at 560℃ in propane dehydrogenation reaction of the catalyst. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] The target catalyst is Ru 1 Co 2 / SiO 2 , the Ru loading is 1%, and the molar ratio of Ru to Co is 1:2.
[0038] Step 1: Weigh 0.0516g RuCl 3 ·3H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added dropwise to the solution to form Ru(OH) 3 Precipitation, continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH 3 ) 6 3+ Exist in the form of complexes.
[0039] Step 2: Weigh 0.0942g CoCl 2 6H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added to the solution to form a green precipitate of cobalt hydroxide. Ammonia water was continued to be added until the solid dissolved to form a purple-red solution. At this time, Co was converted into Co(NH 3 ) 6 2+ Exist in the form of complexes.
[0040] Step 3: Mix the solutions obtained in step 1 and step 2, mix evenly by ultrasonication for 5-10 minutes, continue to drop ammonia water, and adjust the pH value of the solution to 10-11. Weigh 2.0 g SiO 2 The mixed solution was added dropwise onto the carrier, stirring while adding to make the load uniform. Subsequently, it was dried in an oven at 60°C for 48h, and then heated at 650°C and 20% H 2 / N 2 The reduction was carried out in the atmosphere for 4 h, the gas flow rate was 40 mL / min, and the atmosphere furnace heating rate was 5 °C / min, and Ru was finally obtained. 1 Co 2 / SiO 2 Nano alloy catalyst.
[0041] Example 2
[0042] The target catalyst is Ru 1 Cu 5 / Al 2 O 3 , the Ru loading is 1%, and the molar ratio of Ru to Cu is 1:5.
[0043] Step 1: Weigh 0.0516g RuCl 3 ·3H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added dropwise to the solution to form Ru(OH) 3 Precipitation, continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH 3 ) 6 3+ Exist in the form of complexes.
[0044] Step 2: Weigh 0.1693g CuCl 2 ·2H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added to the solution to form a blue flocculent precipitate of copper hydroxide. Ammonia water was added until the solid dissolved to form a blue transparent solution. At this time, Cu was converted into Cu(NH 3 ) 6 2+ Exist in the form of complexes.
[0045] Step 3: Mix the solutions obtained in step 1 and step 2, mix evenly by ultrasonication for 5-10 minutes, continue to drop ammonia water, and adjust the pH value of the solution to 10-11. Weigh 2.0g Al 2 O 3 The mixed solution was added dropwise onto the support, stirring while adding to ensure uniform loading. Subsequently, the mixture was dried in an oven at 80°C for 24 h, and then heated at 600°C with 10% H 2 / N 2 The reduction was carried out in the atmosphere for 4 h, the gas flow rate was 20 mL / min, and the atmosphere furnace heating rate was 2 °C / min, and Ru was finally obtained. 1 Cu 5 / Al 2 O 3 Nano alloy catalyst.
[0046] Example 3
[0047] The target catalyst is Ru 1 Ni 2 / Al 2 O 3 , the Ru loading amount is 0.5%, and the molar ratio of Ru to Ni is 1:2.
[0048] Step 1: Weigh 0.0258g RuCl 3 ·3H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added dropwise to the solution to form Ru(OH) 3 Precipitation, continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH 3 ) 6 3+ Exist in the form of complexes.
[0049] Step 2: Weigh 0.047g NiCl 2 6H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added to the solution to form a white powdery precipitate of nickel hydroxide. Ammonia water was continued to be added until the solid dissolved to form a green transparent solution. At this time, Ni was converted into Ni(NH 3 ) 6 2+ Exist in the form of complexes.
[0050] Step 3: Mix the solutions obtained in step 1 and step 2, mix evenly by ultrasonication for 5-10 minutes, continue to drop ammonia water, and adjust the pH value of the solution to 10-11. Weigh 2.0g Al 2 O 3 The mixed solution was added dropwise onto the support, stirring while adding to ensure uniform loading. Subsequently, the mixture was dried in an oven at 80°C for 24 h, and then heated at 600°C with 10% H 2 / N 2 The reduction was carried out in the atmosphere for 4 h, the gas flow rate was 30 mL / min, and the atmosphere furnace heating rate was 5 °C / min, and finally Ru1Ni 2 / SiO 2 Nano alloy catalyst.
[0051] Example 4
[0052] The target catalyst is Ru 1 Co 5 / C, the Ru loading is 2%, and the molar ratio of Ru to Co is 1:5.
[0053] Step 1: Weigh 0.0516g RuCl 3 ·3H 2 O was dissolved in 2 mL of deionized water, and 25% ammonia water was added dropwise to the solution to form Ru(OH) 3 Precipitation, continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH 3 ) 6 3+Exist in the form of complexes.
[0054] Step 2: Weigh 0.2356g CoCl 2 6H 2 O was dissolved in 5 mL of deionized water, and 25% ammonia water was added to the solution to form a green precipitate of cobalt hydroxide. Ammonia water was continued to be added until the solid dissolved to form a purple-red solution. At this time, Co was converted into Co(NH 3 ) 6 2+ Exist in the form of complexes.
[0055] Step 3: Mix the solutions obtained in step 1 and step 2, mix evenly by ultrasonication for 5-10 minutes, continue to add ammonia water, and adjust the solution pH>10. Weigh 1.0g of carbon carrier, add it to the mixed solution under magnetic stirring, stir and load for 2 hours, and then centrifuge. Then, dry it in an oven at 60℃ for 24h, and then heat it at 700℃ and 10% H 2 / N 2 The reduction was carried out in the atmosphere for 4 h, the gas flow rate was 20 mL / min, and the atmosphere furnace heating rate was 2 °C / min, and Ru was finally obtained. 1 Co 5 / C nano alloy catalyst.
[0056] The catalysts obtained in Examples 1-4 above were characterized:
[0057] Figure 1 The Ru prepared in Example 1 1 Co 2 / SiO 2 Electron microscope photo of the catalyst. Figure 2 The Ru prepared in Example 1 1 Co 2 / SiO 2 The particle size statistics of the catalyst are as follows: Figure 1-2 It can be seen that the RuCo nanoparticles in the obtained supported catalyst are well dispersed on the carrier surface, the particle size is uniform, and the particle size is small, with an average particle size of 3.6 nm.
[0058] Figure 3 Single metal Ru / SiO 2 Catalyst and Ru prepared in Example 1 1 Co 2 / SiO 2 In situ infrared spectrum of CO of the catalyst, curve 1 is single metal Ru / SiO 2 Catalyst, curve 2 is the Ru prepared in Example 1 1 Co 2 / SiO 2 Compared with single metal Ru, Ru1 Co 2 / SiO 2 The CO linear adsorption peak of Ru in the catalyst (2050 cm -1 ) intensity is enhanced and a certain degree of blue shift occurs, indicating that a RuCo alloy is formed, the Ru continuous sites are separated, and Co transfers electrons to Ru.
[0059] Figure 4 The Ru prepared in Example 2 1 Cu 5 / Al 2 O 3 Electron microscope photo of the catalyst. Figure 5 The Ru prepared in Example 2 1 Cu 5 / Al 2 O 3 The particle size statistics of the catalyst are as follows: Figure 4-5 It can be seen that the RuCu nanoparticles in the obtained supported catalyst are evenly dispersed on the support surface, the particle size distribution range is narrow, and the particle size is small, with an average particle size of 4.7 nm.
[0060] Figure 6 The Ru prepared in Example 3 1 Ni 2 / Al 2 O 3 Electron microscope photo of the catalyst. Figure 7 The Ru prepared in Example 3 1 Ni 2 / Al 2 O 3 The particle size statistics of the catalyst are as follows: Figure 6-7 It can be seen that the RuNi nanoparticles in the obtained supported catalyst are well dispersed on the carrier surface, the particle size is uniform, and the particle size is small, with an average particle size of 4.1 nm.
[0061] Figure 8 The Ru prepared in Example 4 1 Co 5 Electron microscope photo of / C catalyst, Fig. 9 The Ru prepared in Example 4 1 Co 5 / C catalyst particle size statistics 9, from Figure 8-9 It can be seen that the RuCo nanoparticles in the obtained supported catalyst are well dispersed on the carrier surface, the particle size is uniform, and the particle size is small, with an average particle size of 3.4 nm.
[0062] Fig.10 Ru / SiO 2 Catalyst, Ru in Example 1 1 Co2 / SiO 2 Catalyst and Ru in Example 2 1 Cu 5 / Al 2 O 3 The curve of propane conversion rate of the catalyst in propane dehydrogenation reaction at 560℃ versus reaction time. Curve 1 represents Ru / SiO 2 Catalyst, curve 2 represents Ru in Example 1 1 Co 2 / SiO 2 Catalyst, curve 3 represents Ru in Example 2 1 Cu 5 / Al 2 O 3 catalyst;
[0063] from Fig.10 It can be seen that with Ru / SiO 2 The catalyst prepared by this method has better activity and stability than Ru / SiO 2 The initial conversion rate of the catalyst was 18.5%, and it was only 11.8% after 60 min of reaction. 1 Co 2 / SiO 2 Catalyst and Ru in Example 2 1 Cu 5 / Al 2 O 3 The initial conversion rates of the catalysts were 24.1% and 24.9%, respectively. After 60 min of reaction, the conversion rates were 18.5% and 20.3%, respectively.
[0064] Fig.11 Ru / SiO 2 Catalyst, Ru in Example 1 1 Co 2 / SiO 2 Catalyst and Ru in Example 2 1 Cu 5 / Al 2 O 3 The change curve of propylene selectivity of catalyst in propane dehydrogenation reaction at 560℃ with time, where curve 1 represents Ru / SiO 2 Catalyst, curve 2 represents the Ru in Example 1 1 Co 2 / SiO 2 Catalyst, curve 3 represents Ru in Example 2 1 Cu 5 / Al 2 O 3 catalyst;
[0065] from Fig.11 It can be seen that the catalyst has a high selectivity for propylene. 1 Co 2 / SiO 2 Catalyst and Ru prepared in Example 2 1 Cu 5 / Al 2 O 3 After the catalyst reaction stabilized, the selectivity was >90%.
[0066] Application Example 1:
[0067] The catalyst of Example 1-2 was used to evaluate the propane dehydrogenation reaction performance. The evaluation device was a fixed bed microreactor. The reaction conditions and operation steps were as follows:
[0068] The reaction tube was a quartz tube with a length of 30 cm and an inner diameter of 1 cm. The generated gas products were analyzed online by a Shimadzu gas chromatograph (GC-2014C) equipped with a PLOT capillary column (0.53 mm × 50 m) and a hydrogen flame ionization detector. The reaction pressure was atmospheric pressure. 200 mg of the catalyst was weighed and mixed evenly with 1.8 g of quartz sand (40-70 mesh). Before the reaction, the sample was heated at 600 °C with 10% H 2 / N 2 After pretreatment for 30 min, a mixed gas with a total flow rate of 50 mL / min (containing 1.25% propane, 1.25% hydrogen and balance nitrogen) was introduced for reaction at a space velocity of 3000 h -1 Then, the temperature was lowered to 560℃ under nitrogen purge to start the reaction. The total flow rate of the reaction gas was 50mL / min, containing 2.5% C 3 H 8 and balance N 2 The propane conversion rate, propylene selectivity and deactivation constant of the propane catalyst at 550°C are shown in Table 1:
[0069] Table 1 Propane conversion, propylene selectivity and deactivation constant results of propane catalyst at 550℃
[0070]
[0071] The comparative sample is Pt / SiO reported in J.Am.Chem.Soc.2018,140,11674-11679. 2 The catalyst has a propane dehydrogenation reaction performance at 550° C. The Pt catalyst is a commonly used propane dehydrogenation catalyst. Compared with the comparative example, the RuM catalyst prepared in the present invention has better activity and selectivity.
[0072] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A supported RuM nano alloy catalyst, characterized in that: The supported RuM nano alloy catalyst comprises the following components, which are expressed in atomic molar percentage as follows: x M y / ZT; A RuM alloy structure is formed in the supported RuM nanoalloy catalyst, and the two elements are evenly distributed; Wherein, M is the second metal, ZT represents a carrier, and the ZT is any one of SiO2, Al2O3, SBA-15 molecular sieve, ZSM-5 molecular sieve, SUZ-4 molecular sieve, SAPO-34 molecular sieve, and mesoporous carbon; Ru x M y is the active component, x / y is the molar ratio of Ru to M, in the range of 0.1-10; The supported RuM nano-alloy catalyst adjusts the pH of the metal precursor solution with ammonia water, and forms an ammonia complex with metal ions, and then uses the strong electrostatic adsorption theory to uniformly adsorb the positively charged metal precursor on the surface of the carrier enriched with negative charges, and is obtained through atmosphere reduction.
2. A supported RuM nano alloy catalyst according to claim 1, characterized in that: The M is one of transition metals including Cu, Co, Ni and Ag.
3. A supported RuM nano alloy catalyst according to claim 1, characterized in that: Ru x M y The particle size is 2-5 nm.
4. A supported RuM nano alloy catalyst according to claim 1, characterized in that: The molar ratio of Ru to M is 0.1-10.
5. A supported RuM nano alloy catalyst according to claim 1, characterized in that: The Ru loading amount is 0.1-10%, and the loading amount is the mass percentage of metal Ru in the carrier.
6. A method for preparing the supported RuM nano alloy catalyst according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Weigh RuCl3 and dissolve it in deionized water. Add 25% ammonia water to the solution to form Ru(OH)3 precipitate. Continue to add ammonia water until the solid dissolves to form a light yellow transparent solution. At this time, the Ru precursor is Ru(NH3)6 3+ Exist in the form of complexes; S2, weigh the second metal M precursor and dissolve it in deionized water, add ammonia water with a mass concentration of 25% to the solution to form the second metal hydroxide precipitate, continue to add ammonia water until the solid is dissolved to form a transparent solution, at this time, the second metal M precursor is M(NH3)6 x+ Exist in the form of complexes; S3, the solutions obtained in step S1 and step S2 are mixed, and the mixture is uniformly mixed by ultrasonication for 5-10 minutes, and ammonia water is continuously added dropwise, and the negative charge concentration on the surface of the carrier is regulated by adjusting the pH of the solution, and the mixed solution is added dropwise onto the carrier by utilizing the mutual attraction of the enriched negative charge on the surface of the carrier to the ammonia complex with positive charge, and then dried in an oven at 60-100°C for 12-24h, and then reduced at 400-800°C in a 5-40% H2 / N2 atmosphere for 2-6h, wherein the gas flow rate is 20-80mL / min, and the atmosphere furnace heating rate is 2-10°C / min, to obtain Ru x M y / ZT nano alloy catalyst.
7. The method for preparing a supported RuM nano alloy catalyst according to claim 6, characterized in that: The volume of deionized water in step S1 is between 1-5 ml.
8. The method for preparing a supported RuM nano-alloy catalyst according to claim 6, characterized in that: The volume of deionized water in step S2 is between 1-5 ml.
9. The method for preparing a supported RuM nano alloy catalyst according to claim 6, characterized in that: In step S3, the solution pH is determined according to the zero charge point pH of the carrier. When the solution pH is greater than the zero charge point, the surface of the carrier is negatively charged.