A method for screening DLP light-curing 3D printing parameters of composite materials

By controlling the exposure intensity and exposure time, combined with Lambert-Bill’s theorem fitting, DLP photocuring 3D printing parameters are optimized, solving the printing problems of high-solid content and high-refractive index composites, and improving printing accuracy and quality.

CN118181762BActive Publication Date: 2024-12-06SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410279151.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-12-06
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

In DLP photocuring 3D printing, the printing parameters of high solids content and high refractive index 0-3 composite materials are difficult to balance, resulting in problems with printing accuracy and curing depth, affecting the printability and mechanical characteristics of the material.

Method used

By controlling the exposure intensity and exposure time, measuring the curing depth and beyond width, fit the relationship curve using the Lambert-Bill theorem, determine the optimal exposure intensity, light energy and printing thickness, calculate the optimal single-layer exposure time, and optimize the composite material Print parameters.

Benefits of technology

Effective printing parameters screening of 0-3 type composite materials with high solid content and high refractive index fillers is realized, printing accuracy and quality are improved, and bonding between layers and light penetration are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118181762B_ABST
    Figure CN118181762B_ABST
Patent Text Reader

Abstract

The present application relates to a method for screening DLP photocuring 3D printing parameters of composite materials, and belongs to the field of additive manufacturing technology. A method for screening DLP photocuring 3D printing parameters of composite materials, comprising: (1) printing multiple first test areas to obtain a first curing depth and a first excess width; (2) determining the optimal exposure intensity through the relationship among exposure intensity, first curing depth, first excess width, and first light energy; (3) based on the optimal exposure intensity, printing multiple second test areas to obtain a second curing depth and a second excess width; determining the optimal light energy and the optimal curing depth through the relationship among the second curing depth, second excess width, and second light energy; (4) obtaining the optimal printing thickness based on the optimal curing depth; (5) obtaining the optimal single-layer exposure time based on the optimal exposure intensity and the optimal light energy. Provide a reference for the actual printing parameters of the composite material to obtain a better printing effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of additive manufacturing technology, and in particular to a method for screening DLP light-curing 3D printing parameters of composite materials. Background Art

[0002] DLP (Digital Light Processing) is an additive manufacturing technology based on digital light processing. The basic principle is that digital light sources are projected layer by layer on the surface of liquid photosensitive resin in the form of surface light, and then cured layer by layer. Different from the single spot moving curing molding of SLA (Stereolithography) 3D printing technology, DLP's 3D printing technology can cure the entire layer of resin raw materials at one time, with higher printing efficiency. DLP technology uses a high-resolution DMD (Digital Micromirror Device) as a mask, allowing high-energy ultraviolet light sources to selectively pass through the DMD mask to cure the resin near the release film. Then the printing platform is lifted, and the uncured liquid resin flows between the printing platform and the release film, and then drops to a suitable position so that the light source can continue to cure the resin material of the adjacent layers. The reciprocating cycle finally forms complex parts. Because DMD has high resolution and each pixel can be individually controlled "on and off", DLP printing technology has high printing accuracy. Studying how to adjust the light-curing additive manufacturing parameters such as the exposure time of the first layer, the exposure number of the base layer, and the exposure time of each subsequent layer during printing can achieve the curing of different photosensitive materials.

[0003] DLP is known for its fast production speed, high resolution and relatively simple machine maintenance. It has become the preferred method for manufacturing ceramic-polymer composites, but the development of ceramic-polymer composites compatible with DLP technology has been slow. The main challenge lies in the difference in physical and chemical properties between fillers and substrates in composites. The refractive index of ceramic particle fillers and resin matrix is ​​very different, which will produce significant light scattering at their interface during printing, thus increasing the complexity of the printing process. Due to the scattering effect, key process parameters such as light energy, exposure intensity, exposure time and layer thickness are interrelated, which poses a challenge to finding the optimal parameters for DLP 3D printing. Higher light energy can deepen the curing depth, but also expand the curing area, affecting the surface finish and printing accuracy. Sufficient curing depth is essential for strong interlayer adhesion. Therefore, sufficient curing depth is the key to ensure the printability of the material, while the minimum overrun width is a necessary condition for maintaining printing accuracy. In addition, higher solid content will enhance the mechanical and piezoelectric properties of the composite, but will have an adverse effect on the penetration of light, which may further lead to incomplete curing and printing failure. For example, the refractive index of piezoelectric ceramics such as lead zirconate titanate (PZT) and barium titanate (BTO) (2.66 and 2.4, respectively) is much higher than that of polymer resins (usually less than 1.6) and common ceramics such as alumina and zirconia (refractive index is 1.77 and 2.17, respectively). This characteristic usually leads to a narrow printing process window for piezoelectric materials, making the optimization of the DLP printing process of piezoelectric ceramic-polymer composites more complicated. The printing of 0-3 type composites with high solid content and high refractive index fillers is very difficult, and several key process parameters are very difficult to balance.

[0004] Common strategies for DLP process optimization aim to broaden the process window, thereby simplifying the selection of printing parameters for piezoelectric composites. These methods include using vacuum conditions during printing, promoting polymerization by reducing oxygen interference, and formulating chemical mixtures to optimize performance at low filler content. However, these traditional methods often require expensive materials, elaborate settings, or complex chemical processing, while the highly coupled parameters of high-filler content materials are not addressed. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the embodiments of the present application includes providing a method for screening DLP light-curing 3D printing parameters of composite materials, so as to improve the current problem that it is very difficult to print 0-3 type composite materials with high solid content and high refractive index fillers, and several key process parameters are very difficult to balance.

[0006] In a first aspect, the present application provides a method for screening DLP light-curing 3D printing parameters of a composite material, comprising:

[0007] (1) printing a plurality of first test areas by controlling exposure intensity and exposure time with gradient variations, respectively, to obtain a first curing depth and a first excess width of each first test area;

[0008] (2) respectively obtaining a first relationship among exposure intensity, a first curing depth, and a first light energy, and a second relationship among exposure intensity, a first excess width, and the first light energy; and determining an optimal exposure intensity based on the first relationship and the second relationship;

[0009] (3) Based on the optimal exposure intensity, the exposure time of the plurality of second test areas is controlled to be changed in a gradient manner for printing, and the second curing depth and the second excess width of each second test area are obtained respectively; a third relationship between the second curing depth, the second excess width and the second light energy is obtained, and the optimal light energy is determined based on the third relationship, and then the optimal curing depth is determined based on the optimal light energy;

[0010] (4) Obtaining optimal printing thickness based on optimal curing depth;

[0011] (5) Obtain the optimal single-layer exposure time based on the optimal exposure intensity and optimal light energy.

[0012] By controlling the exposure intensity and exposure time for pre-printing, measuring and calculating the curing depth and excess width after printing, and then calculating and determining the estimated optimal exposure intensity, optimal printing thickness and optimal single-layer exposure time parameters based on the relationship between exposure intensity, light energy, curing depth and excess width, it provides a reference value for the actual printing parameters of 0-3 type composite materials with high solid content and high refractive index fillers, and obtains better printing effects.

[0013] In some embodiments of the present application, in step (2), a first relationship curve between exposure intensity, first curing depth and first light energy, and a second relationship curve between exposure intensity, first excess width and first light energy are obtained by fitting the Lambert-Beer theorem; based on the first relationship curve and the second relationship curve, the optimal exposure intensity is determined.

[0014] In some embodiments of the present application, determining the optimal exposure intensity based on the first relationship curve and the second relationship curve includes:

[0015] Based on the first relationship curve, determining a first exposure intensity range when the first curing depth is maximum; based on the second relationship curve, determining a second exposure intensity range when the first excess width does not increase with increasing exposure intensity;

[0016] Based on the first exposure intensity range and the second exposure intensity range, the exposure intensity corresponding to the minimum first excess width or the minimum exposure intensity value in the intersection range of the two is selected as the optimal exposure intensity.

[0017] In some embodiments of the present application, in step (3), a first working curve of the second light energy and the second curing depth, and a second working curve of the second light energy and the second excess width are obtained by fitting the Lambert-Beer theorem, the optimal light energy is determined by the second working curve, and the optimal curing depth is determined by the optimal light energy and the first working curve.

[0018] In some embodiments of the present application, determining the optimal light energy through the second working curve includes: determining the light energy corresponding to the minimum value of the second excess width in the second working curve as the optimal light energy.

[0019] In some embodiments of the present application, the optimal curing depth is determined by the optimal light energy and the first working curve, including: determining the second curing depth corresponding to the optimal light energy in the first working curve as the optimal curing depth.

[0020] In some embodiments of the present application, the optimal printing thickness is calculated in step (4) by the following formula: L≤C d / 2;

[0021] Where, L is the optimal printing thickness, C d For the optimal curing depth.

[0022] The curing depth must be at least twice the printing thickness to allow the UV light to cure the current layer and the previous layer at the same time to ensure the bonding strength between the layers; therefore, the printing thickness is best less than 1 / 2 of the curing depth to ensure better curing effect between layers.

[0023] In some embodiments of the present application, the optimal single-layer exposure time is calculated in step (5) by the following formula: t = E / P;

[0024] Where t is the optimal single-layer exposure time, E is the optimal light energy, and P is the optimal exposure intensity.

[0025] In some embodiments of the present application, the composite material includes a 0-3 type ceramic-polymer composite material.

[0026] In some embodiments of the present application, the 0-3 type ceramic-polymer composite material includes a ceramic material and a photosensitive polymer; and the solid content of the 0-3 type ceramic-polymer composite material is not less than 50%.

[0027] In some embodiments of the present application, a light absorber is added to the composite material; the mass fraction of the light absorber is 1%-2%.

[0028] In some embodiments of the present application, a sunscreen is further added to the composite material; the mass fraction of the sunscreen is 0.1%-0.3%. Adding a sunscreen to the composite material can further improve the printing accuracy and quality of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 A schematic diagram of controlling the exposure intensity of gradient changes by controlling the light machine to output different grayscales provided in an embodiment of the present application.

[0031] Figure 2 A schematic diagram of a first test group after printing and curing provided in an embodiment of the present application; wherein a-gradient grayscale, b-gradient exposure intensity.

[0032] Figure 3 This is the first relationship curve diagram provided in Example 1 of the present application.

[0033] Figure 4 This is a second relationship curve diagram provided in Example 1 of the present application.

[0034] Figure 5 This is a schematic diagram of multiple second test areas after printing and curing provided in an embodiment of the present application.

[0035] Figure 6 The first working curve and the second working curve diagram provided in Example 1 of the present application.

[0036] Figure 7 The first working curve and the second working curve diagram provided in Example 2 of the present application.

[0037] Figure 8 The first working curve and the second working curve diagram provided in Example 3 of the present application.

[0038] Fig. 9 The first working curve and the second working curve diagram provided in Example 4 of the present application.

[0039] Fig.10 The first working curve and the second working curve diagram provided in Example 5 of the present application.

[0040] Fig.11 The first working curve and the second working curve diagram provided in Example 6 of the present application.

[0041] Fig.12 Cross-sectional views after printing at different exposure times provided in Experimental Example 1 of the present application; wherein a-exposure time 6s, b-exposure time 4s, c-exposure time 2s.

[0042] Fig.13 The printed body-centered cubic structure diagram provided for Experimental Example 1 of the present application; wherein a-simulation diagram, b-stereoscopic diagram, c-top view, d-front view.

[0043] Fig.14 This is a cross-sectional view after printing with an exposure time of 10s provided in Experimental Example 2 of the present application.

[0044] Fig.15 This is a printed tensile expansion array structure diagram provided for Experimental Example 2 of the present application; wherein a-simulation diagram, b-stereoscopic diagram, c-top view, d-front view. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0046] The present application embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, comprising:

[0047] (1) The prepared mixed composite material slurry is uniformly coated on a transparent film; wherein the composite material is a 0-3 type ceramic-polymer composite material mixed with a ceramic material and a photosensitive polymer; the solid content of the 0-3 type ceramic-polymer composite material is not less than 50%. The weight ratio of the ceramic material to the photosensitive polymer is 1-3:1. As an example, the weight ratio of the ceramic material to the photosensitive polymer can be but is not limited to 1:1, 1.5:1, 2:1, 2.5:1, 3:1. A photoinitiator with a mass fraction of 1%-2% is added to the composite material for subsequent printing, and the composite material slurry is coated on a plurality of test areas on the transparent film. The number of test areas can be set according to the test needs and is not specifically limited.

[0048] As an example, the photoinitiator may be, but is not limited to, IRGACURE 819 (phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide) or LAP (phenyl (2,4,6-trimethylbenzoyl) lithium phosphate). The photoinitiator may be selected according to different composite materials and the wavelength of ultraviolet light of the device.

[0049] In other embodiments, in order to further improve the printing accuracy and quality, a sunscreen can be added to the composite material; the mass fraction of the sunscreen is 0.1%-0.3%. As an example, the mass fraction of the sunscreen can be, but not limited to, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%. As an example, the sunscreen can be, but not limited to, Sudan red, lemon yellow, and carmine. The sunscreen can be selected according to different composite materials and the wavelength of the ultraviolet light of the equipment.

[0050] (2) multiple groups of first test groups are set, and multiple first test areas are set in each first test group; the exposure intensity and exposure time of the multiple first test areas in each group are controlled in a gradient manner, so that the first light energy (light energy = exposure intensity × exposure time) of each first test area in each group is basically equal, and the first light energy between the multiple first test groups forms a gradient change, and printing is performed to obtain the first curing depth and the first excess width of each first test area; wherein the exposure intensity of the gradient change is 0.5-55mW / cm 2 The exposure time of the gradient change is 1-900s. The light energy of each first test area in each group differs by 1-200mJ / cm 2 The first light energy of the gradient change is 57-2200mJ / cm 2 .

[0051] (3) A first relationship curve among the exposure intensity, the first curing depth and the first light energy of the plurality of first test groups is obtained by fitting the Lambert-Beer theorem formula (1), and a second relationship curve among the exposure intensity, the first excess width and the first light energy of the plurality of first test groups is obtained by fitting the Lambert-Beer theorem formula (2); wherein the Lambert-Beer theorem formula (1) is: In the formula, C d is the curing depth, D p is the penetration depth, E d is the minimum energy required for the resin to change from liquid to solid, E0 is the energy density on the surface of the material; Lambert-Beer theorem formula (3) is Where W ex To exceed the width, S w is the width sensitivity, E0 is the energy density on the surface of the material, and E w is the width critical energy.

[0052] Based on the first relationship curve, determining a first exposure intensity range when the first curing depth is maximum; based on the second relationship curve, determining a second exposure intensity range when the first excess width does not increase with increasing exposure intensity;

[0053] Based on the first exposure intensity range and the second exposure intensity range, the exposure intensity corresponding to the minimum first excess width or the minimum exposure intensity value in the intersection range of the two is selected as the optimal exposure intensity. As an example, when the first excess widths corresponding to the intersection ranges of the first exposure intensity range and the second exposure intensity range are the same, the minimum exposure intensity value in the intersection range of the two is determined to be the optimal exposure intensity.

[0054] (4) Based on the optimal exposure intensity, the exposure time of the plurality of second test areas is controlled to be changed in a gradient manner for printing, so as to obtain a second curing depth and a second excess width of each second test area;

[0055] The first working curve of the second light energy and the second curing depth is obtained by fitting the above-mentioned Lambert-Beer theorem formula (1), and the second working curve of the second light energy and the second excess width is obtained by fitting the above-mentioned Lambert-Beer theorem formula (2); wherein the exposure time of the gradient change is 0.5-105s.

[0056] The light energy corresponding to the minimum value of the second excess width in the second working curve is determined as the optimal light energy; and the second curing depth corresponding to the optimal light energy in the first working curve is determined as the optimal curing depth.

[0057] (5) Based on the optimal curing depth, the optimal printing thickness is calculated by the following formula: L ≤ C d / 2; where L is the optimal printing thickness, C d For the optimal curing depth.

[0058] (6) Based on the optimal exposure intensity and the optimal light energy, the optimal single-layer exposure time is calculated by the following formula: t = E / P; wherein t is the optimal single-layer exposure time, E is the optimal light energy, and P is the optimal exposure intensity.

[0059] In some embodiments of the present application, the first curing depth and the second curing depth are calculated by the following formula: d =C2-C1, where C d is the curing depth, C2 is the total thickness of the cured sample and film, and C1 is the film thickness.

[0060] In some embodiments of the present application, the first excess width and the second excess width are calculated by the following formula: Where W ex To exceed the width, W cure is the actual curing width, W design is the desired curing width.

[0061] In some embodiments of the present application, the optimal exposure intensity, optimal printing thickness, and optimal single-layer exposure time obtained according to the screening method of the DLP light-curing 3D printing parameters of the above-mentioned composite materials are estimated reference parameters of the DLP light-curing 3D printing parameters of the actual composite materials. The DLP light-curing 3D printing parameters of the actual composite materials can adjust the above-mentioned optimal exposure intensity, optimal printing thickness, and optimal single-layer exposure time within a certain range according to actual goals.

[0062] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0063] Example 1

[0064] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, comprising:

[0065] (1) mixing piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry in a weight ratio of 1:1, and adding 1.5% of a photoinitiator IRGACURE 819, wherein the polyurethane acrylate slurry is a mixture of polyurethane acrylate and acryloyl morpholine in a weight ratio of 2:1, to form a composite material slurry with a solid content of 50%, and uniformly coating the composite material slurry on a transparent film to form a plurality of first test areas and a second test area;

[0066] (2) Five first test groups are set, each of which has seven first test areas. For each of the seven first test areas, the light machine is controlled to output different grayscales to control the exposure intensity of the gradient change (see Figure 1 As shown in Table 1, the exposure time of the seven first test areas in each group is controlled to change gradually, so that the first light energy of each first test area in each group is substantially equal, and the first light energy between the multiple first test groups forms a gradient change, as shown in Table 1, and printing is performed. The test area after printing and curing is as shown in Table 1. Figure 2 For example, the first curing depth of each first test area is calculated by the following formula: C d =C2-C1, where C d is the curing depth, C2 is the total thickness of the cured sample and the film, C1 is the film thickness; the first excess width of each first test area is calculated by the following formula: Where W ex To exceed the width, W cure is the actual curing width, W design is the desired curing width; the results are shown in Tables 2 and 3;

[0067] Table 1 Printing conditions of the first test group

[0068]

[0069]

[0070] Table 2 First curing depth of the first test group (μm)

[0071] <![CDATA[Exposure intensity (mW / cm 2 )]]> Group 1 Group 2 Group 3 Group 4 Group 5 55 37 59 63 82 97 45 42 56 66 75 96 31 38 57 66 74 92 21 37 55 62 65 80 12 36 54 60 65 75 6 32 53 60 61 64 2.3 26 47 48 55 59

[0072] Table 3 The first excess width of the first test group (μm)

[0073] <![CDATA[Exposure intensity (mW / cm 2 )]]> Group 1 Group 2 Group 3 Group 4 Group 5 55 125 295 780 1865 4725 45 120 345 685 2280 4135 31 120 340 690 1975 4810 21 85 290 545 920 3650 12 50 245 530 1040 2255 6 20 200 470 850 1155 2.3 20 135 260 410 630

[0074] (3) According to the average first light energy data and exposure intensity in Table 1 and the first curing depth data in Table 2, the Lambert-Beer theorem formula (1) In the formula, C d is the curing depth, D p is the penetration depth, E d is the minimum energy required for the resin to change from liquid to solid, E0 is the energy density on the surface of the material, and the first relationship curves among the exposure intensity, the first curing depth and the first light energy of the first test group of 5 groups are obtained by fitting; Figure 3 As shown;

[0075] According to the average first light energy data and exposure intensity in Table 1 and the first excess width data in Table 3, the Lambert-Beer theorem formula (2) is used to calculate Where W ex To exceed the width, S w is the width sensitivity, E0 is the energy density on the surface of the material, and E w is the width critical energy, and the second relationship curves among the exposure intensity, the first excess width and the first light energy of the five first test groups are obtained by fitting; Figure 4 As shown;

[0076] Based on the first relationship curve, it is determined that the first exposure intensity range when the first curing depth is the maximum is 55 mW / cm 2 Based on the second relationship curve, it is determined that the second exposure intensity range when the first excess width does not increase with the increase of exposure intensity is 45mW / cm 2 and 55mW / cm 2 ;

[0077] Based on the first exposure intensity range and the second exposure intensity range, the exposure intensity corresponding to the minimum first excess width in the intersection range of the two is selected as the optimal exposure intensity of 55 mW / cm 2 ;

[0078] (4) Based on the optimal exposure intensity of 55mW / cm 2, set 7 second test areas, control the exposure time of gradient changes in the 7 second test areas respectively as shown in Table 4, print, and calculate the second curing depth of each second test area by the following formula: C d =C2-C1, where C d is the curing depth, C2 is the total thickness of the cured sample and the film, C1 is the film thickness; the second excess width of each second test area is calculated by the following formula: Where W ex To exceed the width, W cure is the actual curing width, W design is the desired curing width; the results are shown in Tables 5 and 6;

[0079] Table 4 Printing conditions of the second test area

[0080]

[0081]

[0082] Table 5 Second curing depth of the second test area (μm)

[0083] Second test area Exposure time(s) Second curing depth (μm) 1 0.5 46 2 1.5 68 3 3 80 4 8 91 5 18 105 6 44 118 7 105 116

[0084] Table 6 Second excess width of the second test area (μm)

[0085] Second test area Exposure time(s) Second excess width (μm) 1 0.5 200 2 1.5 305 3 3 2050 4 8 3345 5 18 5290 6 44 7760 7 105 9700

[0086] According to the second light energy data in Table 4 and the second curing depth data in Table 5, the first working curve of the second light energy and the second curing depth is obtained by fitting the Lambert-Beer theorem formula (1); and according to the second light energy data in Table 4 and the second excess width data in Table 6, the second working curve of the second light energy and the second excess width is obtained by fitting the Lambert-Beer theorem formula (2); Figure 6 As shown;

[0087] The optimal light energy is determined to be 60 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy 60mJ / cm 2 The second curing depth corresponding to the first working curve is determined to be the optimal curing depth of 60 μm;

[0088] (5) Based on the optimal curing depth of 60 μm, the optimal printing thickness is calculated to be ≤30 μm by the following formula: L≤C d / 2; where L is the optimal printing thickness, C d For the optimal curing depth;

[0089] (6) Based on the optimal exposure intensity of 55mW / cm2 And the optimal light energy is 60mJ / cm 2 The optimal single-layer exposure time is calculated to be 1 s by the following formula: t=E / P; wherein t is the optimal single-layer exposure time, E is the optimal light energy, and P is the optimal exposure intensity.

[0090] Example 2

[0091] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, comprising:

[0092] (1) mixing piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry at a weight ratio of 1.5:1, and adding 1.5% of the mass fraction of the photoinitiator IRGACURE 819, wherein the polyurethane acrylate slurry is a mixture of polyurethane acrylate and acryloyl morpholine at a weight ratio of 2:1, to form a composite material slurry with a solid content of 60%, and uniformly coating the composite material slurry on a transparent film to form a plurality of first test areas and a second test area;

[0093] (2) The optimal exposure intensity is determined to be 55 mW / cm by the same method as steps (2) and (3) in Example 1. 2 ;

[0094] (3) Based on the optimal exposure intensity of 55mW / cm 2 , set 7 second test areas, control the exposure time of gradient change for the 7 second test areas respectively as shown in Table 7, and print, and the test areas after printing and curing are as shown in Table 7. Figure 5 Example, the second curing depth of each second test area is calculated by the same method as in Example 1; the results are shown in Tables 8 and 9;

[0095] Table 7 Printing conditions of the second test area

[0096]

[0097] Table 8 Second curing depth of the second test area (μm)

[0098] Second test area Exposure time(s) Second curing depth (μm) 1 1 52 2 3 59 3 7 66 4 16 67 5 37 74 6 89 80 7 211 82

[0099] Table 9 Second excess width of the second test area (μm)

[0100]

[0101]

[0102] According to the second light energy data in Table 7 and the second curing depth data in Table 8, the first working curve of the second light energy and the second curing depth is obtained by fitting the Lambert-Beer theorem formula (1); and according to the second light energy data in Table 7 and the second excess width data in Table 9, the second working curve of the second light energy and the second excess width is obtained by fitting the Lambert-Beer theorem formula (2); Figure 7 As shown;

[0103] The optimal light energy is determined to be 80 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy 80mJ / cm 2 The second curing depth corresponding to the first working curve is determined to be the optimal curing depth of 50 μm;

[0104] (4) Based on the optimal curing depth of 50 μm, the optimal printing thickness is calculated to be ≤25 μm using the same method as in Example 1;

[0105] (5) Based on the optimal exposure intensity of 55mW / cm 2 and optimal light energy 80mJ / cm 2 The optimal single-layer exposure time calculated in the same way as in Example 1 is 1.5 s.

[0106] Example 3

[0107] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, which differs from Embodiment 2 in that:

[0108] (1) mixing piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry in a weight ratio of 2:1 to form a composite material slurry with a solid content of 66.7%;

[0109] (2) obtaining a first working curve of the second light energy and the second curing depth, and a second working curve of the second light energy and the second excess width, such as Figure 8 As shown;

[0110] The optimal light energy is determined to be 90 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy of 90mJ / cm 2 The corresponding second curing depth in the first working curve is determined to be the optimal curing depth of 41 μm;

[0111] (3) Based on the optimal curing depth of 41 μm, the optimal printing thickness is calculated to be ≤20.5 μm;

[0112] (4) Based on the optimal exposure intensity of 55mW / cm 2 And the optimal light energy is 90mJ / cm2 The optimal single-layer exposure time is calculated to be 1.6s.

[0113] Example 4

[0114] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, which differs from Embodiment 2 in that:

[0115] (1) mixing piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry in a weight ratio of 2.5:1 to form a composite material slurry with a solid content of 71.4%;

[0116] (2) obtaining a first working curve of the second light energy and the second curing depth, and a second working curve of the second light energy and the second excess width, such as Fig. 9 As shown;

[0117] The optimal light energy is determined to be 70 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy of 70mJ / cm 2 The second curing depth corresponding to the first working curve is determined to be the optimal curing depth of 30 μm;

[0118] (3) The optimal printing thickness is calculated to be ≤15 μm based on the optimal curing depth of 30 μm;

[0119] (4) Based on the optimal exposure intensity of 55mW / cm 2 And the optimal light energy is 70mJ / cm 2 The optimal single-layer exposure time is calculated to be 1.3s.

[0120] Example 5

[0121] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, which differs from Embodiment 2 in that:

[0122] (1) mixing piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry in a weight ratio of 3:1 to form a composite material slurry with a solid content of 75%;

[0123] (2) obtaining a first working curve of the second light energy and the second curing depth, and a second working curve of the second light energy and the second excess width, such as Fig.10 As shown;

[0124] The optimal light energy is determined to be 65 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy 65mJ / cm 2 The corresponding second curing depth in the first working curve is determined to be the optimal curing depth of 23 μm;

[0125] (3) The optimal printing thickness is calculated to be ≤11.5 μm based on the optimal curing depth of 23 μm;

[0126] (4) Based on the optimal exposure intensity of 55mW / cm 2 and optimal light energy 65mJ / cm 2 The optimal single-layer exposure time is calculated to be 1.2s.

[0127] Example 6

[0128] This embodiment provides a method for screening DLP light-curing 3D printing parameters of a composite material, which differs from Embodiment 2 in that:

[0129] (1) piezoelectric ceramic PZT-5H powder and polyurethane acrylate slurry were mixed in a weight ratio of 1:1, and 1.5% by weight of photoinitiator IRGACURE 819 was added, and 0.1% by weight of Sudan IV pigment was added to the slurry to form a composite material slurry with a solid content of 50%;

[0130] (2) obtaining a first working curve of the second light energy and the second curing depth, and a second working curve of the second light energy and the second excess width, such as Fig.11 As shown;

[0131] The optimal light energy is determined to be 900 mJ / cm based on the light energy corresponding to the second excess width being the minimum value 0 in the second working curve. 2 ; Based on the optimal light energy of 900mJ / cm 2 The corresponding second curing depth in the first working curve is determined to be the optimal curing depth of 38 μm;

[0132] (3) The optimal printing thickness is calculated to be ≤19 μm based on the optimal curing depth of 38 μm;

[0133] (4) Based on the optimal exposure intensity of 55mW / cm 2 And the optimal light energy is 900mJ / cm 2 The optimal single-layer exposure time was calculated to be 16 s.

[0134] Test Example 1

[0135] This test example is based on the optimal exposure intensity of 55mW / cm 2 , the optimal printing thickness is ≤30μm, and the optimal single-layer exposure time is 1s; since the bonding force between the current layer and the previous layer needs to be guaranteed during actual printing, the actual printing thickness is determined to be slightly smaller than the calculated printing thickness value, and the actual exposure time is appropriately adjusted to ensure a better curing effect; first determine that the actual printing thickness is 20μm;

[0136] Since the exposure time will affect the excess width, the exposure intensity is 55mW / cm 2 , the printing thickness is 20 μm, and the composite material in Example 1 is printed by controlling different exposure times of 2s, 4s, and 6s according to actual conditions. The cross-section after printing is as follows Fig.12 As shown, it can be seen that the excess width is the smallest when the exposure time is 2s, so the actual exposure time is determined to be 2s;

[0137] The final exposure intensity was 55mW / cm 2 , print thickness 20μm, exposure time 2s print body-centered cubic (BCC) structure, the results are as follows Fig.13 shown.

[0138] Depend on Fig.13 By comparing b, c, d and a, it can be seen that the estimated optimal exposure intensity, optimal printing thickness and optimal single-layer exposure time parameters are determined by the calculation determined by the screening method of DLP light-curing 3D printing parameters of the composite material of the present application, which provides a reference value for the actual printing parameters of 0-3 type composite materials with high solid content and high refractive index fillers, and obtains more accurate and higher quality printing effects.

[0139] Test Example 2

[0140] This test example is based on the optimal exposure intensity of 55mW / cm 2 , the optimal printing thickness is ≤19μm, and the optimal single-layer exposure time is 16s; since the bonding force between the current layer and the previous layer needs to be guaranteed during actual printing, the actual printing thickness is determined to be slightly smaller than the calculated printing thickness value to ensure a better curing effect; the actual printing thickness is determined to be 15μm, and according to the actual goal, the priority is given to improving the printing accuracy, and the actual exposure time is determined to be 10s;

[0141] Since the exposure time will affect the excess width, the exposure intensity is 55mW / cm 2 , printing thickness of 15 μm, exposure time of 10 s, the composite material in Example 6 was printed, and the cross section after printing was as follows Fig.14 As shown, after adding the light absorber to the composite material, the excess width after printing is almost 0, and the printing accuracy is high;

[0142] The final exposure intensity was 55mW / cm 2 , printing thickness 15μm, exposure time 10s printing auxetic array structure, the results are as follows Fig.15 shown.

[0143] Depend on Fig.15From the comparison of b, c, d and a, it can be seen that the estimated optimal exposure intensity, optimal printing thickness and optimal single-layer exposure time parameters are determined by the calculation determined by the screening method of DLP light-curing 3D printing parameters of the composite material of the present application, which provides a reference value for the actual printing parameters of 0-3 type composite materials with high solid content and high refractive index fillers with added light absorbers, and obtains more accurate and higher quality printing effects. Adding a sunshade to the composite material can further improve the printing accuracy and quality.

[0144] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.

Claims

1. A method for screening DLP light-curing 3D printing parameters of composite materials, characterized in that: include: (1) printing a plurality of first test areas by controlling exposure intensity and exposure time with gradient variations, respectively, to obtain a first curing depth and a first excess width of each of the first test areas; (2) obtaining a first relationship curve among the exposure intensity, the first curing depth and the first light energy, and a second relationship curve among the exposure intensity, the first excess width and the first light energy respectively by fitting the Lambert-Beer theorem; Determining an optimal exposure intensity based on the first relationship curve and the second relationship curve, wherein determining the optimal exposure intensity comprises: Based on the first relationship curve, determining a first exposure intensity range when the first curing depth is maximum; based on the second relationship curve, determining a second exposure intensity range when the first excess width does not increase as the exposure intensity increases; Based on the first exposure intensity range and the second exposure intensity range, selecting the exposure intensity corresponding to the minimum first excess width or the minimum exposure intensity value in the intersection range of the two as the optimal exposure intensity; (3) Based on the optimal exposure intensity, the exposure time of the plurality of second test areas is controlled to change with gradients for printing, and the second curing depth and the second excess width of each second test area are obtained respectively; a third relationship between the second curing depth, the second excess width and the second light energy is obtained, and the optimal light energy is determined based on the third relationship, and then the optimal curing depth is determined based on the optimal light energy, specifically comprising: obtaining a first working curve of the second light energy and the second curing depth and a second working curve of the second light energy and the second excess width by fitting the Lambert-Beer theorem, determining the light energy corresponding to the minimum value of the second excess width in the second working curve as the optimal light energy, and then determining the optimal curing depth based on the second curing depth corresponding to the optimal light energy in the first working curve; (4) Based on the optimal curing depth, the optimal printing thickness is obtained, and the optimal printing thickness is calculated by the following formula: L≤C d / 2; where L is the optimal printing thickness, C d For the optimal curing depth; (5) Based on the optimal exposure intensity and the optimal light energy, the optimal single-layer exposure time is obtained, and the optimal single-layer exposure time is calculated by the following formula: t=E / P; wherein t is the optimal single-layer exposure time, E is the optimal light energy, and P is the optimal exposure intensity.

2. The screening method according to claim 1, characterized in that The composite material comprises a 0-3 type ceramic-polymer composite material; the 0-3 type ceramic-polymer composite material comprises a ceramic material and a photosensitive polymer; the solid content of the 0-3 type ceramic-polymer composite material is not less than 50%.

3. The screening method according to claim 2, characterized in that A light absorber is added into the composite material; the mass fraction of the light absorber is 1%-2%.

4. The screening method according to claim 3, characterized in that A sunscreen is also added to the composite material; the mass fraction of the sunscreen is 0.1%-0.3%.