A kind of low-impurity ferric phosphate and its preparation method and application

Through step-by-step oxidation process and pH adjustment of the phosphoric acid solution, the precipitation problem of impurity elements in wet phosphoric acid is solved, the utilization rate of phosphorus and the purity of iron phosphate are improved, the production cost and impurity content are reduced, and it is suitable for high-performance iron phosphate. Preparation of lithium positive electrode material.

CN118183665BActive Publication Date: 2024-12-03HUBEI HONGRUN HIGH-TECH NEW MATERIALS CO LTD

Patent Information

Application Number
CN202410432820.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-11
Publication Date
2024-12-03
Estimated Expiration
2044-04-11

AI Technical Summary

Technical Problem

In the existing iron phosphate synthesis method, wet phosphoric acid contains a large number of impurity elements (such as Al, Mg, Mn, Zn), which causes phosphorus elements and impurity cations to form phosphate precipitation and filter out, resulting in phosphorus resources. Waste and low phosphorus comprehensive utilization rate.

Method used

Using the step-by-step oxidation process, by adjusting the pH value and temperature of the phosphoric acid solution, first deposit aluminum impurities, and then gradually oxidize divalent iron ions through two-step oxidizing agents, inhibit the precipitation of Mg and Mn, improve the utilization rate of phosphorus, and pass The solid-liquid separation, washing and sintering steps provide low-impact anhydrous iron phosphate.

Benefits of technology

The utilization rate of phosphorus in wet phosphoric acid is significantly improved, the production cost of iron phosphate is reduced, and the iron phosphate impurity content is low, which improves the purity and electrochemical properties of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118183665B_ABST
    Figure CN118183665B_ABST
Patent Text Reader

Abstract

The present application provides a low-impurity iron phosphate and its preparation method and application, which belongs to the field of high-purity iron phosphate preparation. The preparation method includes: mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution, adjusting the pH of the phosphoric acid solution to heat and age to obtain an aged slurry, filtering to obtain a phosphate solution, adding water and a first oxidant to obtain a phosphate aqueous solution containing the first oxidant; mixing a ferrous sulfate solution with a phosphate aqueous solution containing the first oxidant to obtain a first slurry; heating and aging to obtain a second slurry after the first slurry changes color; separating the second slurry from the solid and liquid, and washing, drying and sintering the obtained solid material in turn to obtain low-impurity iron phosphate. In the present application, wet-process phosphoric acid is used as a raw material, which greatly improves the utilization rate of phosphorus in wet-process phosphoric acid, and the prepared anhydrous iron phosphate has a low impurity content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to low-impurity ferric phosphate and a preparation method and application thereof. Background Art

[0002] At present, the mainstream process routes for preparing iron phosphate are the following three methods:

[0003] (1) Sodium method: Add a mixed solution of sodium hydroxide, phosphoric acid and hydrogen peroxide dropwise to a divalent iron compound solution to prepare ferric phosphate;

[0004] (2) Ammonium method: Add a mixed solution of ammonium dihydrogen phosphate or diammonium hydrogen phosphate and hydrogen peroxide dropwise to a divalent iron compound solution to prepare ferric phosphate;

[0005] (3) Iron method: Use high-purity phosphoric acid and elemental iron to prepare ferrous dihydrogen phosphate solution, and then use hydrogen peroxide as an oxidant and precipitant to prepare ferric phosphate.

[0006] The mainstream iron phosphate synthesis methods in the aforementioned industry mostly use wet phosphoric acid as raw material. Wet phosphoric acid contains a large amount of impurity elements such as Al, Mg, Mn, and Zn. Before being used to prepare iron phosphate, the wet phosphoric acid needs to be impurity-removed. During the impurity removal process, a large amount of phosphorus elements and impurity cations are easily formed into phosphate precipitation and filtered out, resulting in a low comprehensive utilization rate of phosphorus, thereby causing a waste of phosphorus resources.

[0007] Therefore, there is an urgent need to develop a low-cost, low-phosphorus loss preparation method that can significantly improve the utilization rate of phosphorus while obtaining high-purity iron phosphate.

[0008] In view of this, the present invention is proposed. Summary of the invention

[0009] In view of the technical problems existing in the background technology, the present application provides a low-impurity ferric phosphate and a preparation method and application thereof, aiming to reduce phosphorus loss and improve phosphorus utilization while ensuring the purity of the ferric phosphate product.

[0010] In a first aspect, the present invention provides a method for preparing low-impurity ferric phosphate, comprising:

[0011] Mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution, adjusting the pH of the phosphoric acid solution to 2.0-3.0, and then heating and aging to obtain an aged slurry;

[0012] filtering the aged slurry to obtain a phosphate solution, and then adding water and a first oxidant to obtain a phosphate aqueous solution containing the first oxidant;

[0013] mixing the ferrous sulfate solution with the phosphate aqueous solution containing the first oxidant to obtain a first slurry;

[0014] The first slurry is heated and aged, and after the first slurry changes color, a second oxidant is added to the first slurry to obtain a second slurry;

[0015] The second slurry is subjected to solid-liquid separation, and the obtained solid material is sequentially washed, dried and sintered to obtain low-impurity iron phosphate.

[0016] In the technical scheme of the embodiment of the present application, wet phosphoric acid is used as raw material, wet phosphoric acid and water are mixed to obtain a phosphoric acid solution, and the pH value of the phosphoric acid solution is adjusted to 2.0-3.0 and then heated and aged. Due to the difference in the solubility product of iron phosphate and aluminum phosphate, aluminum is first deposited to achieve the purpose of removing aluminum. However, the prepared phosphate solution still contains magnesium and manganese impurities, and then an oxidant is added in two steps to oxidize divalent iron ions. The step-by-step oxidation scheme is used to make a trace amount of trivalent iron ions in the system, suppressing the precipitation of Mg and Mn, greatly improving the utilization rate of phosphorus in wet phosphoric acid, and the prepared anhydrous iron phosphate impurity content is low. In addition, compared to the prior art using high-purity monoammonium phosphate / diammonium or phosphoric acid as a phosphorus source, the wet phosphoric acid raw material cost used in the embodiment of the present application is lower, which can significantly reduce the process cost.

[0017] In some embodiments, the first oxidant and the second oxidant are independently selected from one of hydrogen peroxide, ammonium persulfate, and sodium persulfate.

[0018] In the technical solution of the embodiment of the present application, the provided first oxidant and second oxidant raw materials are easily available and are both suitable for oxidizing divalent iron ions.

[0019] In some embodiments, the molar ratio of the first oxidant to the ferrous ions in the ferrous sulfate solution is (0.7-0.9):2; and / or

[0020] The molar ratio of the second oxidant added dropwise to the first slurry to the ferrous ions in the ferrous sulfate solution is (0.2-0.5):2;

[0021] The molar ratio of the total amount of the first oxidant and the second oxidant to the ferrous ions in the ferrous sulfate solution is (1.1-1.4):2.

[0022] In this embodiment, by regulating the amount of the first oxidant and the second oxidant added in the two-step oxidation, the amount of the first oxidant is 0.7 to 0.9 times the total amount of divalent iron completely oxidized, and the amount of the second oxidant is 0.2 to 0.5 times the total amount of divalent iron completely oxidized. At the same time, the total amount of the oxidants added twice is controlled to be slightly larger than the theoretical amount, so as to more accurately control the reaction process, fully convert the divalent iron into trivalent iron, and reduce the introduction of manganese and magnesium elements in the product.

[0023] In some embodiments, the step of obtaining an aged slurry from wet-process phosphoric acid comprises:

[0024] Mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution containing 5% to 10% by mass of phosphorus;

[0025] The pH value of the phosphoric acid solution is adjusted to 2.0-3.0, and then the solution is aged by heating to obtain an aged slurry.

[0026] In this embodiment, the phosphoric acid solution can more fully remove aluminum impurities after temperature aging by regulating the concentration of the phosphoric acid solution, thereby preventing aluminum ions from entering the subsequent ferrous iron oxidation stage and interfering with the formation of ferric iron precipitation, thereby reducing the introduction of impurity elements in the product ferric phosphate.

[0027] In some embodiments, the temperature of the temperature-raising aging is 85° C. to 95° C., and the time of the temperature-raising aging is 1 h to 4 h.

[0028] In this embodiment, by precisely controlling the operating temperature and aging time of the temperature rise aging, aluminum can be fully deposited to achieve a better aluminum removal effect.

[0029] In some embodiments, in the phosphate aqueous solution containing the first oxidant, the molar concentration of phosphate is 1.0 mol / L to 2.5 mol / L.

[0030] In this embodiment, by adjusting the concentration of the phosphate aqueous solution, it is beneficial to control the reaction rate during the synthesis of iron phosphate, so that the reaction rate will not be too fast, thereby improving the uniformity of the product.

[0031] In some embodiments, the phosphate aqueous solution containing the first oxidant is added dropwise to the ferrous sulfate solution for 10 min to 60 min, and the reaction is continued for 10 min to 60 min after the addition is completed.

[0032] In this embodiment, ferrous sulfate solution is used as the base liquid, and the reaction is carried out by dropwise adding a phosphate aqueous solution. The first oxidant is added slowly, which is beneficial to controlling the reaction rate and allowing the iron phosphate to precipitate evenly.

[0033] In some embodiments, the step of obtaining the second slurry from the first slurry includes: heating the first slurry for aging at a temperature of 80°C to 95°C, adding a second oxidant to the first slurry after the first slurry changes color, and then keeping the first slurry warm for 30 minutes to 90 minutes to obtain the second slurry.

[0034] In this embodiment, the first slurry is heated and aged to undergo a crystal transformation, from an amorphous phase to a crystalline state of ferric phosphate dihydrate, thereby changing the color of the first slurry. After the remaining divalent iron ions are oxidized, a second oxidant is added dropwise to continue the oxidation reaction.

[0035] In some embodiments, washing is a countercurrent wash; and / or

[0036] The drying temperature is 90°C to 110°C and the drying time is 2h to 12h; and / or

[0037] The sintering temperature is 550°C to 650°C, and the sintering time is 1h to 8h.

[0038] In this embodiment, after solid-liquid separation of the second slurry, solid iron phosphate material is obtained, and residual phosphate ions on the surface are removed by washing, and washing water is removed by drying, and an anhydrous iron phosphate product is obtained after sintering.

[0039] In some embodiments, the raw material of the ferrous sulfate solution is titanium dioxide byproduct; and / or

[0040] The molar concentration of the ferrous sulfate solution is 0.5 mol / L to 1.5 mol / L.

[0041] In this embodiment, by regulating the source of ferrous sulfate solution, the raw material is easily available and the process cost is reduced; by regulating the concentration of divalent iron ions, the reaction rate of generating ferric phosphate is not too fast, which is conducive to obtaining an ferric phosphate product with a more uniform particle size.

[0042] In the second aspect, an embodiment of the present application provides a low-impurity iron phosphate, which is prepared by the preparation method in any of the above-mentioned embodiments, wherein the content of impurity element Mg in the prepared low-impurity iron phosphate is ≤40ppm, and the content of impurity element Mn is ≤60ppm.

[0043] In the technical solution of the embodiment of the present application, by optimizing the preparation process of iron phosphate and suppressing the precipitation of impurities such as Mg and Mn through a two-step oxidation process, the utilization rate of phosphorus in wet phosphoric acid is greatly improved, and the prepared anhydrous iron phosphate has a low impurity content.

[0044] On the third aspect, an embodiment of the present application provides a lithium iron phosphate positive electrode material, which is prepared using the above-mentioned low-impurity iron phosphate as a precursor. Since the impurity content in the iron phosphate is low, it is beneficial to improve the purity of the lithium iron phosphate positive electrode material product, thereby facilitating obtaining better electrochemical performance.

[0045] In a fourth aspect, an embodiment of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode active layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises the lithium iron phosphate positive electrode material in the above embodiment. Due to the improvement of the electrochemical performance of the lithium iron phosphate positive electrode material, the positive electrode plate is endowed with excellent electrochemical performance.

[0046] In a fifth aspect, the present application provides a secondary battery, comprising the above-mentioned positive electrode sheet. Based on the excellent electrochemical performance of the positive electrode sheet, the electrochemical performance of the secondary battery product can be further improved.

[0047] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0049] Figure 1 A schematic flow chart of a method for preparing low-impurity ferric phosphate provided in an embodiment of the present application;

[0050] Figure 2 A schematic diagram of the process flow of a method for preparing low-impurity ferric phosphate provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0051] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0053] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0054] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0055] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0056] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0057] In the description of the embodiments of the present application, if technical terms such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. appear to indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0058] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, if technical terms such as "installed", "connected", "connected", "fixed" and the like appear, they should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0059] At present, the mainstream synthesis methods of iron phosphate all require the removal of impurities from wet-process phosphoric acid to prepare industrial-grade phosphate or phosphoric acid with low impurities, and then use the refined high-purity phosphate or phosphoric acid as the phosphorus source to prepare iron phosphate. It is known that wet-process phosphoric acid contains a large amount of impurity elements such as Al, Mg, Mn, and Zn. In the process of removing the above impurities, a large amount of phosphorus elements and impurity cations will form phosphate precipitation and be filtered out, which directly leads to a large waste of phosphorus resources.

[0060] In order to improve the comprehensive utilization rate of phosphorus in the raw materials, the embodiment of the present application provides a method for preparing low-impurity ferric phosphate, which avoids the process route of Mg and Mn precipitation through a step-by-step oxidation scheme, greatly improves the utilization rate of phosphorus in wet-process phosphoric acid, and reduces the amount of alkali used, reduces the production cost of ferric phosphate, and the prepared anhydrous ferric phosphate has a low impurity content.

[0061] Please refer to Figure 1 In a first aspect, the present invention provides a method for preparing low-impurity ferric phosphate, comprising the following steps:

[0062] S1, mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution, and adjusting the pH of the phosphoric acid solution to 2.0-3.0, and then heating and aging to obtain an aged slurry;

[0063] S2, filtering the aged slurry to obtain a phosphate solution, and then adding water and a first oxidant to obtain a phosphate aqueous solution containing the first oxidant;

[0064] S3, mixing the ferrous sulfate solution with the phosphate aqueous solution containing the first oxidant to obtain a first slurry;

[0065] S4, heating the first slurry for aging, and after the first slurry changes color, adding a second oxidant to the first slurry to obtain a second slurry;

[0066] S5. The second slurry is subjected to solid-liquid separation, and the obtained solid material is sequentially washed, dried and sintered to obtain low-impurity iron phosphate.

[0067] Further, in step S1 of the present application, a wet-process phosphoric acid sample is used as a raw material, and an aluminum removal process is first performed to obtain an aged slurry. Specifically, the preparation method of the phosphate aqueous solution containing the first oxidant includes: mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution containing 5% to 10% phosphorus by mass; adjusting the pH value of the phosphoric acid solution to 2.0 to 3.0, and then heating and aging to obtain an aged slurry.

[0068] Specifically, the mass fraction of phosphorus in the phosphoric acid solution can be 5%, 8%, 10%, etc. When adjusting the pH value of the phosphoric acid solution, the alkali solution used can be ammonia water, sodium hydroxide solution, etc., but is not limited thereto. By adjusting the amount of alkali solution added, the pH value of the system after pH adjustment can be 2.0, 2.5, 3.0, etc.

[0069] In some embodiments, the temperature of the temperature-raising aging is controlled to be 85°C to 95°C, and the time of the temperature-raising aging is 1h to 4h. After the pH value is adjusted to meet the requirements, the temperature-raising aging is performed, and the temperature of the aging can be controlled to be 85°C, 90°C, 95°C, etc., and the aging time can be 1h, 2h, 3h, 4h, etc.

[0070] In step S2, the aged slurry is filtered to obtain a phosphate solution; a first oxidant and water are added to the phosphate solution, and the concentration of phosphorus is adjusted to obtain a phosphate aqueous solution containing the first oxidant.

[0071] It should be noted that the pH value of the phosphoric acid solution is adjusted to 2.0-3.0. After the temperature is increased, due to the difference in solubility product between iron phosphate and aluminum phosphate, aluminum is first deposited to achieve the purpose of removing aluminum. The reaction slurry after temperature increase and aging is subjected to solid-liquid separation by filtering and other means to obtain aluminum-containing filter residue and phosphate solution. The aluminum-containing filter residue enters other processes to recover aluminum. The phosphate solution is mixed with the first oxidant and water so that the concentration of phosphate and the amount of the first oxidant meet the process requirements to obtain a phosphate aqueous solution containing the first oxidant.

[0072] By using the embodiment of the present invention, only aluminum impurities in wet-process phosphoric acid are separated, so that a large amount of Mg and Mn impurities in the wet-process phosphoric acid exist in the form of ions, thereby avoiding the consumption of phosphorus elements by phosphate formed by Mg and Mn impurities, and improving the utilization rate of phosphorus. Compared with the process route for preparing monoammonium phosphate from wet-process phosphoric acid (pH value 4.0-5.0), the embodiment of the present invention adjusts the pH value of phosphate (2.0-3.0) to be lower, thereby reducing the amount of ammonia water used.

[0073] In some embodiments, in the phosphate aqueous solution containing the first oxidant, the molar concentration of phosphate is 1.0mol / L to 2.5mol / L, such as 1.0mol / L, 1.5mol / L, 2.0mol / L, 2.5mol / L. By regulating the concentration of the phosphoric acid solution and the phosphate aqueous solution, it is beneficial to control the reaction rate during the synthesis of iron phosphate, so that the reaction rate will not be too fast, and the uniformity of the product is improved. The amount of the first oxidant added is determined according to the content of ferrous ions in the ferrous sulfate solution, and the molar ratio of the first oxidant in the phosphate aqueous solution to the ferrous ions in the ferrous sulfate solution is (0.7 to 0.9): 2, such as 0.7:2, 0.8:2, 0.9:2, etc. That is to say, when preparing the phosphate aqueous solution containing the first oxidant, the amount of the first oxidant added is controlled to be 0.7 to 0.9 times the total amount of completely oxidized divalent iron.

[0074] In some embodiments, the first oxidant is selected from one of hydrogen peroxide, ammonium persulfate and sodium persulfate, and can be any one of the above, all of which are suitable for oxidizing divalent iron ions.

[0075] Specifically, before step S3, a ferrous sulfate solution is also required. In the present application, the source of ferrous sulfate is not limited. For example, it can be a ferrous sulfate solution after the byproduct of titanium dioxide is refined and impurities are removed. The ferrous sulfate solution can be diluted with pure water. By regulating the source of the ferrous sulfate solution, the raw materials are easily available and the process cost is reduced. Among them, the molar concentration of divalent iron in the prepared ferrous sulfate solution can be 0.5mol / L to 1.5mol / L, such as 0.5mol / L, 1.0mol / L, 1.5mol / L, etc. The reaction rate of generating ferric phosphate can be regulated by regulating the concentration of divalent iron ions, so as to facilitate obtaining an ferric phosphate product with a more uniform particle size.

[0076] Specifically, in step S3, the phosphate aqueous solution containing the first oxidant can be added dropwise to the ferrous sulfate solution, the addition time is 10min to 60min, and the reaction is continued for 10min to 60min after the addition is completed, so that the first oxidant is fully reacted. Preferably, the ferrous sulfate solution is used as the base liquid, and the phosphate aqueous solution is added dropwise to react, so that the first oxidant is slowly added, which is conducive to controlling the reaction rate and making the iron phosphate precipitate uniformly. Among them, the addition time of the phosphate aqueous solution containing the first oxidant can be 10min, 20min, 30min, 40min, 50min, 60min, etc., and the reaction time after the addition is completed can be 10min, 20min, 30min, 40min, 50min, 60min, etc.

[0077] It should be noted that in the first stage oxidation reaction, the amount of the first oxidant is 0.7 to 0.9 times the total amount of completely oxidized ferrous iron. The amount of the first oxidant is not enough to completely oxidize the ferrous iron ions. The ferrous iron is fully oxidized only after the subsequent second stage oxidation reaction.

[0078] Specifically, in step S4, the first slurry is heated and aged, and after the first slurry changes color, a second oxidant is added dropwise to the first slurry to carry out a two-stage oxidation reaction, and a second slurry is obtained after the reaction. The reason for the discoloration of the first slurry is mainly due to the transformation of iron phosphate from an amorphous phase to a crystalline state of iron phosphate dihydrate. In the embodiment of the present invention, the oxidant is added in two steps, so that a trace amount of trivalent iron ions are present in the system during the color change process to inhibit the precipitation of impurity ions, so that the overall process does not require a complicated impurity removal process, and greatly improves the utilization rate of phosphorus in wet-process phosphoric acid.

[0079] In some embodiments, the first oxidant and the second oxidant are independently selected from one of hydrogen peroxide, ammonium persulfate and sodium persulfate. The first oxidant and the second oxidant may be the same or different. When the above oxidants completely oxidize the divalent iron ions, the molar ratio of the oxidant to the divalent iron ions is 1:2.

[0080] In some embodiments, the molar ratio of the second oxidant added to the first slurry to the ferrous ions in the ferrous sulfate solution is (0.2-0.5):2; at the same time, the molar ratio of the total amount of the first oxidant and the second oxidant to the ferrous ions in the ferrous sulfate solution is controlled to be (1.1-1.4):2. In other words, the total amount of the oxidant used in the two-stage oxidation reaction is slightly excessive, and the amount of the second oxidant added during the two-stage oxidation reaction is 0.2-0.5 times the total amount of completely oxidized divalent iron. By more accurately controlling the reaction process, the divalent iron is fully converted into trivalent iron, while reducing the introduction of manganese and magnesium elements in the ferric phosphate product.

[0081] Specifically, the amount of the second oxidant added to the first slurry is calculated according to the amount of ferrous ions in the prepared ferrous sulfate solution, and the molar ratio of the second oxidant added to the first slurry to the ferrous ions in the ferrous sulfate solution can be controlled to be 0.1:2, 0.2:2, 0.3:2, 0.4:2, 0.5:2, etc. In other words, the amount of the second oxidant required for the second-stage oxidation reaction process can be calculated based on the theoretical amount of the second oxidant required to completely oxidize the ferrous ions in the ferrous sulfate solution, so that the amount of the second oxidant added to the first slurry is 0.2 to 0.5 times the theoretical amount.

[0082] Specifically, the total amount of the first oxidant and the second oxidant can also be calculated according to the amount of ferrous ions in the prepared ferrous sulfate solution, and the molar ratio of the total amount of the oxidant added in the two steps to the ferrous ions in the ferrous sulfate solution can be 1.1:2, 1.2:2, 1.3:2, 1.4:2, etc. When the molar ratio of the oxidant to the divalent iron ion is 1:2, the oxidant can completely oxidize the divalent iron ion, and the total amount of the oxidant used in the two-step reaction controlled by the embodiment of the present invention is 1.1 to 1.4 times the theoretical amount.

[0083] In some embodiments, the first slurry is heated and aged, and the aging temperature is controlled to be 80°C to 95°C. After the first slurry changes from pale white to pale pink, a peristaltic pump can be used to drip a second oxidant into the slurry after the color change is completed, and the temperature is kept for 30min to 90min after the second oxidant is added. The first slurry is heated and aged to undergo a crystal transformation, from an amorphous phase to a crystalline state of iron phosphate dihydrate, thereby changing the color of the first slurry, and then the second oxidant is dripped to continue the oxidation reaction.

[0084] Specifically, when the first slurry is heated and aged, the aging temperature can be controlled to be 80°C, 85°C, 90°C, 95°C, etc., and the insulation time after the second oxidant is added can be 30min, 40min, 50min, 60min, 70min, 80min, 90min, etc.

[0085] Specifically, in step S5, iron phosphate dihydrate in the second slurry is separated, and low-impurity iron phosphate can be prepared after processes such as impurity removal and sintering.

[0086] In some embodiments, the second slurry is subjected to solid-liquid separation, and the obtained solid material is washed, dried and sintered in sequence. The phosphate ions remaining on the surface are removed by washing, the washing water is removed by drying, and an anhydrous iron phosphate product is obtained after sintering.

[0087] In some embodiments, the washing may be countercurrent washing, so that the solid material can be fully contacted with the washing water, so that the phosphate ions remaining on the surface can be fully removed, and the washing water is removed by drying, and an anhydrous iron phosphate product is obtained after sintering.

[0088] In some embodiments, the drying temperature is 90°C to 110°C, and the drying time is 2h to 12h. Within this drying temperature and time range, the surface washing water can be more fully removed without affecting the crystal morphology of the iron phosphate. Specifically, the drying temperature can be 90°C, 95°C, 100°C, 105°C, 110°C, and the drying time can be 2h, 5h, 8h, 10h, 12h, etc.

[0089] In some embodiments, the sintering temperature is 550°C to 650°C, and the sintering time is 1h to 8h. Within this sintering temperature and sintering time range, the dihydrated ferric phosphate can lose crystal water to obtain an anhydrous ferric phosphate product. Specifically, the sintering temperature can be 550°C, 600°C, 650°C, etc., and the sintering time can be 1h, 3h, 5h, 8h, etc.

[0090] Based on the above analysis, please refer to Figure 2 The main steps of the preparation method provided in the present application are as follows: adding water to wet-process phosphoric acid to dissolve it to obtain a phosphoric acid solution, adding ammonia water to the phosphoric acid solution to adjust the pH value to meet the requirements, and then heating and aging to obtain an aged aluminum slurry; after solid-liquid separation of the aged aluminum slurry, aluminum-containing filter residue and refined phosphate solution are obtained, the refined phosphate solution and a first oxidant are mixed to obtain a phosphate aqueous solution containing hydrogen peroxide, and the phosphate aqueous solution containing hydrogen peroxide is added dropwise to a prepared ferrous sulfate solution for a first oxidation reaction to obtain a first slurry; heating and aging the first slurry, and after color change, a second oxidant is added dropwise for a second oxidation reaction to obtain a second slurry; after solid-liquid separation and washing of the second slurry, ferric phosphate dihydrate is obtained; the ferric phosphate dihydrate is dried and sintered to obtain a low-impurity anhydrous ferric phosphate product.

[0091] In the second aspect, the embodiment of the present application provides a low-impurity iron phosphate, which is prepared by the above-mentioned preparation method, wherein the content of impurity element Mg in the prepared low-impurity iron phosphate is ≤40ppm, and the content of impurity element Mn is ≤60ppm. By optimizing the preparation process of iron phosphate, the precipitation of impurities such as Mg and Mn is suppressed by a two-step oxidation process, the utilization rate of phosphorus in wet-process phosphoric acid is greatly improved, and the prepared anhydrous iron phosphate has a low impurity content.

[0092] It should be noted that "low impurities" means that the impurity content in ferrophosphate products is low, and the main impurities are Mg and Mn, among which the Mg content is ≤40ppm and the Mn content is ≤60ppm. In addition to Mg and Mn, ferrophosphate products also contain other impurities, such as Na, Ni, Pb, etc., but the content is small, generally less than 12ppm.

[0093] In a third aspect, an embodiment of the present application provides a lithium iron phosphate positive electrode material, which is prepared using the low-impurity iron phosphate as a precursor. Exemplarily, the lithium iron phosphate positive electrode material is prepared by ball milling, drying and calcining the low-impurity iron phosphate, lithium salt and carbon source as raw materials.

[0094] Since the impurity content in iron phosphate is low, it is beneficial to improve the purity of lithium iron phosphate positive electrode material products, thereby facilitating the acquisition of better electrochemical performance.

[0095] In a fourth aspect, the present application provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode active layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode active layer comprises the above-mentioned lithium iron phosphate positive electrode material. Due to the improvement of the electrochemical performance of the lithium iron phosphate positive electrode material, the positive electrode sheet is endowed with excellent electrochemical performance.

[0096] In the fifth aspect, the embodiment of the present application provides a secondary battery, including the above-mentioned positive electrode plate, and may also include a negative electrode plate, an electrolyte, a separator, etc., to form a complete battery structure. Based on the excellent electrochemical performance of the positive electrode plate, the electrochemical performance of the secondary battery product can be further improved.

[0097] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.

[0098] Example 1

[0099] This embodiment provides a method for preparing low-impurity ferric phosphate, comprising the following steps:

[0100] (1) Preparation of ferrous sulfate solution: Take the ferrous sulfate solution obtained by refining and removing impurities from the titanium dioxide byproduct, add pure water to prepare a ferrous sulfate solution with a molar concentration of 1.0 mol / L for use.

[0101] (2) Preparation of refined phosphate solution: 484.49 g of wet-process phosphoric acid sample (mass fraction 78.25%, specific composition see Table 1) was taken and pure water was added to prepare a phosphoric acid solution with a phosphorus mass fraction of 8.0%. Ammonia water was added dropwise to the phosphoric acid solution under stirring to adjust the pH value of the system to 2.5. After the pH value adjustment was completed, the reaction solution was heated to 90° C. and aged for 2.0 h. After the aging was completed, the slurry was filtered to obtain a refined phosphate solution.

[0102] The filter residue was dried and weighed to a mass of 31.48 g, and the phosphorus content was detected to be 20.88%. The phosphorus loss was calculated based on the total phosphorus mass taken away by the filter residue, and the phosphorus loss rate was 5.48%.

[0103] (3) Preparation of a phosphate aqueous solution containing a first oxidant: Take the refined phosphate solution in step (2), add pure water and hydrogen peroxide, and the molar ratio of the amount of hydrogen peroxide added to the ferrous ion in the ferrous sulfate solution in step (1) is 0.84:2 (i.e., the ratio of hydrogen peroxide added is 0.84 times the total amount of ferrous iron completely oxidized), and prepare a phosphate solution with a phosphorus molar concentration of 2.0 mol / L for use.

[0104] (4) One-stage oxidation reaction: Start the reactor and stir. Use 200 mL of the ferrous sulfate solution in step (1) as the base liquid and use a peristaltic pump to dropwise add 100 mL of the phosphate aqueous solution containing the first oxidant in step (3) into the reactor over 30 minutes. After the dropwise addition is completed, continue the reaction for 30 minutes to obtain a first slurry.

[0105] (5) Second-stage oxidation reaction: The first slurry of step (4) is heated and aged at a temperature of 90° C. After the reaction slurry changes from pale white to pale pink, hydrogen peroxide is continuously added to the slurry after the color change using a peristaltic pump. The molar ratio of the added hydrogen peroxide to the ferrous ions in the ferrous sulfate solution is 0.36:2 (i.e., the ratio of hydrogen peroxide added is 0.36 times the total amount of ferrous iron to be completely oxidized). After the addition is completed, the temperature is maintained for 60 min to obtain a second slurry.

[0106] (6) Preparation of anhydrous iron phosphate: The second slurry of step (5) was filtered, washed in countercurrent, dried at 95° C. for 6 h, and sintered at 600° C. for 4 h to obtain anhydrous iron phosphate.

[0107] Example 2

[0108] The only difference from Example 1 is the amount of hydrogen peroxide added in step (3) and step (5). Specifically, in step (3) of this embodiment, the molar ratio of the amount of hydrogen peroxide ① added to the ferrous ions in the ferrous sulfate solution in step (1) is 0.7:2; and the molar ratio of the hydrogen peroxide ② added dropwise in step (5) to the ferrous ions in the ferrous sulfate solution is 0.5:2.

[0109] Example 3

[0110] The only difference from Example 1 is the amount of hydrogen peroxide added in step (3) and step (5). Specifically, in step (3) of this embodiment, the molar ratio of the amount of hydrogen peroxide ① added to the ferrous ions in the ferrous sulfate solution in step (1) is 0.9:2; and the molar ratio of the hydrogen peroxide ② added dropwise in step (5) to the ferrous ions in the ferrous sulfate solution is 0.3:2.

[0111] Example 4

[0112] The only difference from Example 1 is the amount of hydrogen peroxide added in step (3) and step (5). Specifically, in step (3) of this embodiment, the molar ratio of the amount of hydrogen peroxide ① added to the ferrous ions in the ferrous sulfate solution in step (1) is 0.8:2; and the molar ratio of the hydrogen peroxide ② added dropwise in step (5) to the ferrous ions in the ferrous sulfate solution is 0.4:2.

[0113] Example 5

[0114] This embodiment provides a method for preparing low-impurity ferric phosphate, comprising the following steps:

[0115] (1) Preparation of ferrous sulfate solution: Take the ferrous sulfate solution obtained by refining and removing impurities from the titanium dioxide byproduct, add pure water to prepare a ferrous sulfate solution with a molar concentration of 0.5 mol / L for use.

[0116] (2) Preparation of refined phosphate solution: 484.49 g of wet-process phosphoric acid sample (mass fraction 78.25%, specific composition see Table 1) was taken and pure water was added to prepare a phosphoric acid solution with a phosphorus mass fraction of 5.0%. Ammonia water was added dropwise to the phosphoric acid solution under stirring to adjust the pH value of the system to 2.0. After the pH value adjustment was completed, the reaction solution was heated to 85° C. and aged for 4.0 h. After the aging was completed, the slurry was filtered to obtain a refined phosphate solution.

[0117] (3) Preparation of a phosphate aqueous solution containing a first oxidant: Take the phosphate solution refined in step (2), add pure water and hydrogen peroxide, and the molar ratio of the amount of hydrogen peroxide added to the ferrous ion in the ferrous sulfate solution in step (1) is 0.7:2 (i.e., the ratio of hydrogen peroxide added is 0.7 times the total amount of ferrous iron to be completely oxidized), and prepare a phosphate solution with a phosphorus molar concentration of 1.0 mol / L for use.

[0118] (4) One-stage oxidation reaction: Start the reactor and stir. Use 200 mL of the ferrous sulfate solution in step (1) as the base liquid and use a peristaltic pump to dropwise add 100 mL of the phosphate aqueous solution containing the first oxidant in step (3) into the reactor over a period of 10 minutes. After the dropwise addition is completed, continue the reaction for 60 minutes to obtain a first slurry.

[0119] (5) Secondary oxidation reaction: The slurry after the reaction in step (4) is heated and aged at a temperature of 80°C. After the reaction slurry changes from pale white to pale pink, a peristaltic pump is used to continue to drip hydrogen peroxide into the slurry after the color change. The molar ratio of the added hydrogen peroxide to the ferrous ion in the ferrous sulfate solution is 0.5:2 (i.e., the ratio of hydrogen peroxide added is 0.5 times the total amount of ferrous iron to be completely oxidized). After the addition is completed, the temperature is maintained for 30 minutes to obtain a second slurry.

[0120] (6) Preparation of anhydrous iron phosphate: The second slurry of step (5) was filtered, washed in countercurrent, dried at 90° C. for 12 h, and sintered at 550° C. for 8 h to obtain anhydrous iron phosphate.

[0121] Example 6

[0122] This embodiment provides a method for preparing low-impurity ferric phosphate, comprising the following steps:

[0123] (1) Preparation of ferrous sulfate solution: Take the ferrous sulfate solution obtained by refining and removing impurities from the titanium dioxide byproduct, add pure water to prepare a ferrous sulfate solution with a molar concentration of 1.5 mol / L for use.

[0124] (2) Preparation of refined phosphate solution: 484.49 g of wet-process phosphoric acid sample (mass fraction 78.25%, specific composition see Table 1) was taken and pure water was added to prepare a phosphoric acid solution with a phosphorus mass fraction of 10.0%. Sodium hydroxide solution was added dropwise to the phosphoric acid solution under stirring to adjust the pH value of the system to 3.0. After the pH value adjustment was completed, the reaction solution was heated to 95° C. and aged for 1.0 h. After the aging was completed, the slurry was filtered to obtain a refined phosphate solution.

[0125] (3) Preparation of a phosphate aqueous solution containing a first oxidant: Take the phosphate solution refined in step (2), add pure water and hydrogen peroxide①, the molar ratio of the amount of hydrogen peroxide added to the ferrous ion in the ferrous sulfate solution in step (1) is 0.9:2 (i.e., the ratio of hydrogen peroxide added is 0.9 times the total amount of ferrous iron to be completely oxidized), and prepare a phosphate solution with a phosphorus molar concentration of 2.5 mol / L for use.

[0126] (4) One-stage oxidation reaction: Start the reactor and stir. Use 200 mL of the ferrous sulfate solution in step (1) as the base liquid and use a peristaltic pump to dropwise add 100 mL of the phosphate aqueous solution containing the first oxidant in step (3) into the reactor over 60 minutes. After the dropwise addition is completed, continue the reaction for 10 minutes to obtain a first slurry.

[0127] (5) Second-stage oxidation reaction: The slurry after the reaction in step (4) is heated and aged at a temperature of 95°C. After the reaction slurry changes from pale white to pale pink, a peristaltic pump is used to continue to drip hydrogen peroxide into the slurry after the color change. The molar ratio of the added hydrogen peroxide to the ferrous ion in the ferrous sulfate solution is 0.3:2 (i.e., the ratio of hydrogen peroxide added is 0.3 times the total amount of ferrous iron to be completely oxidized). After the addition is completed, the temperature is maintained for 90 minutes to obtain a second slurry.

[0128] (6) Preparation of anhydrous iron phosphate: The second slurry of step (5) was filtered, washed in countercurrent, dried at 110° C. for 2 h, and sintered at 650° C. for 1 h to obtain anhydrous iron phosphate.

[0129] Comparative Example 1

[0130] The only difference from Example 1 is that the addition of hydrogen peroxide to the phosphate follows the traditional one-step method, and the ratio of hydrogen peroxide added is 1.2 times the total amount of completely oxidized ferrous iron to ensure that the ferrous iron in the system is completely oxidized. The other steps are the same as those in Example 1. The specific steps are as follows:

[0131] (1) Preparation of ferrous sulfate solution: same as in Example 1.

[0132] (2) Preparation of refined phosphate solution: same as in Example 1.

[0133] (3) Preparation of phosphate: Take the phosphate solution purified in step (2), add pure water and hydrogen peroxide① (the ratio of hydrogen peroxide added is 1.20 times the total amount of completely oxidized divalent iron), and prepare a phosphate solution with a phosphorus molar concentration of 2.0 mol / L for use.

[0134] (4) Synthesis of ferric phosphate: Start the reactor and stir. Use 200 mL of the ferrous sulfate solution prepared in step (1) as the base liquid and use a peristaltic pump to dropwise add 100 mL of the prepared phosphate into the reactor over 30 minutes. After the dropwise addition is completed, continue the reaction for 30 minutes.

[0135] (5) Crystal transformation: The slurry after the reaction in step (4) was aged at a temperature of 90° C. After the reaction slurry changed from pale white to pale pink, the temperature was kept at 90° C. for 60 min.

[0136] (6) Preparation of anhydrous iron phosphate: The slurry after the reaction in step (5) is filtered, countercurrent washed, dried at 95° C. for 6 h, and sintered at 600° C. for 4 h to obtain anhydrous iron phosphate.

[0137] Comparative Example 2

[0138] In the comparative example, the wet-process phosphoric acid adopts the conventional phosphoric acid impurity removal scheme, that is, the wet-process phosphoric acid is first adjusted to a pH value of 7.0, filtered, and then the pH value of the phosphate is adjusted to 2.0-3.0 using refined phosphoric acid. The addition of hydrogen peroxide to the phosphate follows the traditional one-step scheme, and the proportion of hydrogen peroxide added is 1.2 times the total amount of completely oxidized divalent iron to ensure that the divalent iron in the system is completely oxidized. The other steps are the same as in the embodiment, and the specific steps are as follows:

[0139] (1) Preparation of ferrous sulfate solution: take the ferrous sulfate solution obtained by refining and removing impurities from the titanium dioxide byproduct, add pure water to prepare a ferrous sulfate solution with a molar concentration of divalent iron of 1.0 mol / L for use.

[0140] (2) Preparation of refined phosphate solution: 484.49 g of wet-process phosphoric acid sample (mass fraction 78.25%) was taken and pure water was added to prepare a phosphoric acid solution with a phosphorus mass fraction of 8.0%. Ammonia water was added dropwise to the phosphoric acid solution under stirring to adjust the pH value of the system to 7.0. After the pH value adjustment was completed, the reaction solution was heated to 90° C. and aged for 2.0 h. After the aging was completed, the slurry was filtered and the filtrate was adjusted to a pH value of 2.5 using refined phosphoric acid to obtain a refined phosphate solution.

[0141] The filter residue was dried and weighed to 73.01 g, and the phosphorus content was 22.90%. The phosphorus loss was calculated based on the total phosphorus mass taken away by the filter residue, and the phosphorus loss rate was 13.95%.

[0142] (3) Preparation of phosphate: Take the phosphate solution refined in step (2), add pure water and hydrogen peroxide (the ratio of hydrogen peroxide added is 1.20 times the total amount of completely oxidized divalent iron) to prepare a phosphate solution with a phosphorus molar concentration of 2.0 mol / L for use.

[0143] (4) Synthesis of ferric phosphate: Start the reactor and stir. Use 200 mL of the ferrous sulfate solution prepared in step (1) as the base liquid and use a peristaltic pump to dropwise add 100 mL of the prepared phosphate into the reactor over 30 minutes. After the dropwise addition is completed, continue the reaction for 30 minutes.

[0144] (5) Crystal transformation: The slurry after the reaction in step (4) was aged at a temperature of 90° C. After the reaction slurry changed from pale white to pale pink, the temperature was kept at 90° C. for 60 min.

[0145] (6) Preparation of anhydrous iron phosphate: The slurry after the reaction in step (5) is filtered, countercurrent washed, dried at 95° C. for 6 h, and sintered at 600° C. for 4 h to obtain anhydrous iron phosphate.

[0146] In the present application, the composition of the phosphate obtained after refining in step (2) of the test examples and comparative examples was calculated, and the element removal rate and phosphorus loss rate were calculated, and the results are shown in Table 2. The composition and content of the impurity elements of anhydrous iron phosphate prepared in the test examples and comparative examples were shown in Table 3.

[0147] Table 1 Main components of wet phosphoric acid

[0148]

[0149] According to the test results of raw material wet-process phosphoric acid in Table 1, the main impurity components are Al, Mg and Mn.

[0150] Table 2 Phosphorus loss and element detection data of phosphates prepared in Examples and Comparative Examples

[0151]

[0152]

[0153] Table 3 Impurity element detection data of anhydrous iron phosphate prepared in the embodiment and comparative example

[0154]

[0155] It can be found from Table 2 that the method of the embodiment of the present invention can effectively remove Al impurities, with a removal efficiency of up to 97.78%. At the same time, Mg and Mn impurities are retained in the liquid phase in the form of ions, thereby reducing the phosphorus loss rate from 13.95% to 5.48%, with a saving of 8.47%, which can significantly reduce the production cost of iron phosphate and has good economic benefits.

[0156] As can be seen from Table 3, the segmented oxidation scheme provided in the embodiment of the present invention can significantly reduce the Mg and Mn impurity contents in anhydrous ferric phosphate compared to the traditional one-step method for preparing ferric phosphate. The Mg content is reduced from 91.4ppm to 23.2ppm, and the Mn content is reduced from 233.29ppm to 56.47ppm, indicating that the segmented oxidation scheme provided in the embodiment of the present invention can significantly reduce the Mg and Mn contents in anhydrous ferric phosphate.

[0157] In summary, the use of the directional impurity removal-stage oxidation scheme of the present invention can significantly reduce the loss of phosphorus resources and reduce the production cost of iron phosphate; at the same time, the use of the staged oxidation scheme better solves the problem of high Mg and Mn impurity content in the traditional one-step process for preparing iron phosphate, expands the application scenarios of the one-step process for synthesizing iron phosphate, and makes the prepared iron phosphate more suitable for preparing high-performance lithium iron phosphate.

[0158] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A method for preparing low-impurity ferric phosphate, characterized in that: include: Mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution, adjusting the pH of the phosphoric acid solution to 2.0-3.0, and then heating and aging to obtain an aged slurry; filtering the aged slurry to obtain a phosphate solution, and then adding water and a first oxidant to obtain a phosphate aqueous solution containing the first oxidant; Mixing the ferrous sulfate solution with the phosphate aqueous solution containing the first oxidant to obtain a first slurry; The first slurry is heated and aged, and after the first slurry changes color, a second oxidant is added to the first slurry to obtain a second slurry; The second slurry is subjected to solid-liquid separation, and the obtained solid material is sequentially washed, dried and sintered to obtain the low-impurity iron phosphate; The molar ratio of the first oxidant to the ferrous ions in the ferrous sulfate solution is (0.7-0.9):2; The molar ratio of the second oxidant added dropwise to the first slurry to the ferrous ions in the ferrous sulfate solution is (0.2-0.5):2; The molar ratio of the total amount of the first oxidant and the second oxidant to the ferrous ions in the ferrous sulfate solution is (1.1-1.4):

2.

2. The preparation method according to claim 1, characterized in that: The first oxidant and the second oxidant are independently selected from one of hydrogen peroxide, ammonium persulfate and sodium persulfate.

3. The preparation method according to claim 1, characterized in that: The step of obtaining the aged slurry from the wet-process phosphoric acid comprises: Mixing wet-process phosphoric acid and water to obtain a phosphoric acid solution containing 5% to 10% by mass of phosphorus; The pH value of the phosphoric acid solution is adjusted to 2.0-3.0, and then the solution is aged by heating to obtain an aged slurry.

4. The preparation method according to claim 3, characterized in that: The temperature of the heating aging is 85° C. to 95° C., and the time of the heating aging is 1 h to 4 h.

5. The preparation method according to claim 3, characterized in that: In the phosphate aqueous solution containing the first oxidant, the molar concentration of phosphate is 1.0 mol / L to 2.5 mol / L.

6. The preparation method according to claim 1, characterized in that: The phosphate aqueous solution containing the first oxidant is added dropwise to the ferrous sulfate solution for 10 to 60 minutes, and the reaction is continued for 10 to 60 minutes after the addition is completed.

7. The preparation method according to claim 1, characterized in that: The step of obtaining the second slurry from the first slurry includes: heating and aging the first slurry at a temperature of 80°C to 95°C, adding the second oxidant to the first slurry after the first slurry changes color, and then keeping the first slurry warm for 30 minutes to 90 minutes to obtain the second slurry.

8. The preparation method according to claim 1, characterized in that: The washing is a countercurrent washing; and / or The drying temperature is 90°C to 110°C and the drying time is 2h to 12h; and / or The sintering temperature is 550°C to 650°C, and the sintering time is 1h to 8h.

9. The preparation method according to claim 1, characterized in that: The raw material of the ferrous sulfate solution is titanium dioxide byproduct; and / or The molar concentration of the ferrous sulfate solution is 0.5 mol / L to 1.5 mol / L.

Citation Information

Patent Citations

  • Preparation method of low-manganese and low-magnesium iron phosphate

    CN116621141A

  • Method for preparing battery-grade iron phosphate by using phosphorite crude acid

    CN117550575A

Cited By

  • Low-impurity ferric phosphate, and preparation method therefor and use thereof

    EP4656597A1

  • Low-impurity ferric phosphate, and preparation method therefor and use thereof

    WO2025213559A1