A method for efficiently preparing lignin nanoparticles with hollow structure and its application

CN118185078A8Active Publication Date: 2024-11-29NANJING FORESTRY UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410149437.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-11-29
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

Existing technologies have problems such as complex operations, long time consumption, low efficiency and low purity when preparing lignin nanoparticles, and are not effective in drug loading applications, limiting the application of lignin in high-value fields.

Method used

The anti-solvent precipitation method of tetrahydrofuran-water system was used combined with centrifugation method, and uniform lignin nanoparticles with hollow structure were prepared by controlling the rotation speed and classification. On this basis, the efficient loading and simultaneous preparation of the drug vancomycin was achieved.

Benefits of technology

The preparation of lignin nanoparticles with simple operation, less time-consuming and high efficiency has been achieved. It has good antibacterial properties and drug release effect, with a release rate of more than 80%, promoting the high-value utilization of lignin in the field of biomedicine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118185078A8_ABST
    Figure CN118185078A8_ABST
Patent Text Reader

Abstract

The invention discloses a method and application for efficiently preparing lignin nanoparticles with a hollow structure, and belongs to the technical field of material classification and purification. The method comprises the following steps: preparing lignin into a nanoparticle suspension by an anti-solvent precipitation method, and classifying the prepared lignin nanoparticle suspension by controlling the centrifugal speed to obtain lignin nanoparticles with a hollow structure. The method is simple to operate, less time-consuming, highly efficient, green and environmentally friendly, low-cost, and easy to industrialize; at the same time, vancomycin can be loaded by adding drugs in the self-assembly process, providing a new idea for the high-value utilization of lignin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of material classification and purification, and more specifically, relates to a method for efficiently preparing lignin nanoparticles with a hollow structure and an application thereof. Background Art

[0002] Lignin is a natural aromatic polymer with a complex structure, composed of phenylpropane structural units. It is a biomass resource second only to cellulose in nature, with the characteristics of abundant sources, low cost, good biodegradability and reinforcing performance. In addition, its surface contains a large number of functional groups, such as hydroxyl, methoxy, carbonyl, carboxyl, etc., with excellent multifunctionality and potential application value in many fields. It has been used in high-value applications such as adhesives, surfactants, UV shielding and drug transportation. However, at present, the main application of lignin is still as a low-value fuel combustion, and less than 2% of lignin is applied to high-value applications. Due to the complex structure, large molecular weight, poor processability, its own heterogeneity, and poor dispersibility in water, the multi-field application of lignin is seriously restricted.

[0003] Lignin nanoparticles with hollow structures have advantages such as lower mass than solid particles, higher surface area, and structural controllability, and have been widely studied in the fields of antibacterial, filler, and drug delivery. The benzene ring structure and phenol unit of lignin give it excellent antibacterial ability. Compared with the original lignin, lignin nanoparticles (LNPs) have a larger specific surface area and more functional groups are distributed on the surface of lignin particles, making them exhibit better antibacterial properties. In the study of Yang et al., it was found that small-sized lignin nanoparticles can penetrate into bacterial cells and reduce the pH value in bacterial cells, eventually exhausting adenosine triphosphate (ATP) to kill bacteria, confirming that lignin nanoparticles have excellent antibacterial properties. With the breakthrough progress in lignin chemistry, lignin structure, and preparation technology, lignin-based drug carriers have attracted attention in drug transportation due to their natural and non-toxic characteristics. Zhou et al. proposed a simple method for preparing targeted lignin hollow nanoparticles (LHNPs) and achieved the loading and targeted delivery of doxorubicin hydrochloride (DOX). The lignin nanoparticles prepared by this method can respond to external magnetic fields and folate receptors, and their good targeting ability increases cellular uptake.

[0004] Generally, lignins of different molecular weights contain different types and contents of active functional groups. Therefore, if lignin can be graded according to molecular weight and functional group enrichment, and lignin fractions with low polydispersity or high reaction activity can be obtained, it will play an important role in promoting the development and utilization of lignin downstream products. Commonly used lignin classification methods mainly include membrane classification, acid precipitation classification, organic solvent classification, ionic liquid classification and hydrothermal classification. Membrane classification is an important direction of current lignin classification research. It has the advantages of high efficiency, simplicity and no secondary pollution. However, due to expensive equipment, short life, high maintenance and cost, its large-scale application is greatly limited. The acid precipitation classification method has a simple operation process, short reaction time and low energy consumption, but the resulting lignin has low purity compared with other classification methods, and the acid recovery cost is high, which will cause potential pollution. Summary of the invention

[0005] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is to provide a method for efficiently preparing lignin nanoparticles with a hollow structure, which is simple to operate, less time-consuming and highly efficient. Another technical problem to be solved by the present invention is to provide an application of the above lignin nanoparticles with a hollow structure in drug loading.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for efficiently preparing lignin nanoparticles with a hollow structure, comprising: preparing a lignin nanoparticle suspension by an anti-solvent precipitation method of a tetrahydrofuran-water system, and obtaining uniform lignin nanoparticles with a hollow structure by controlling the rotation speed for classification; wherein the uniform lignin nanoparticles with a hollow structure have a hollow structure diameter of 423 to 715 nm, and the hollow structure surface area accounts for 19.98 to 34.3%.

[0008] Preferably, the lignin is amphiphilic lignin. The amphiphilic lignin is crude lignin or purified lignin, and the preparation process of the purified lignin is as follows: the crude lignin is dissolved in a dichloroethane / ethanol solution, and after being fully dissolved, an ether solution is added, and the lignin is fully stirred and precipitated; centrifuged at 8000rpm for 5min, and the precipitate after centrifugation is washed with ether and petroleum ether for 3 times and 1 time respectively, and dried for 12h after washing to obtain purified lignin.

[0009] Preferably, the controlled rotation speed classification is to classify the lignin nanoparticles with and without a hollow structure at a rotation speed of 5000 rpm.

[0010] Preferably, the lignin nanoparticle suspension is prepared directly by using an anti-solvent precipitation method of a tetrahydrofuran-water system without prior classification treatment, wherein tetrahydrofuran is the solvent and the aqueous solution is the anti-solvent.

[0011] The method for efficiently preparing lignin nanoparticles with a hollow structure comprises the following steps:

[0012] 1) dissolving lignin in tetrahydrofuran, and then adding dropwise the aqueous solution and stirring to obtain a lignin nanoparticle suspension;

[0013] 2) centrifuging the prepared lignin nanoparticle suspension at a rotation speed of 1000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain 1000 rpm lignin nanoparticles;

[0014] 3) taking the supernatant after centrifugation at 1000 rpm and continuing to centrifuge at 3000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 3000 rpm;

[0015] 4) taking the supernatant after centrifugation at 3000 rpm and continuing to centrifuge at 5000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 5000 rpm;

[0016] 5) taking the supernatant after centrifugation at 5000 rpm and continuing to centrifuge at 8000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 8000 rpm;

[0017] 6) The supernatant after centrifugation at 8000 rpm is centrifuged again at 10000 rpm, and the precipitate is dried in a vacuum drying oven to obtain lignin nanoparticles at 10000 rpm.

[0018] 6. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 5 is characterized in that the centrifugation time is 5 minutes, the drying temperature in the vacuum drying oven is 40°C, and the drying time is 48 hours.

[0019] The method for efficiently preparing lignin nanoparticles with a hollow structure can prepare lignin nanoparticles with a hollow structure.

[0020] The application of the lignin nanoparticles with a hollow structure in drug loading.

[0021] In the application, lignin and the drug are added into tetrahydrofuran at the same time, and then an aqueous solution is added dropwise to obtain a mixed suspension, and the mixed suspension is centrifuged to obtain drug-loaded lignin nanoparticles.

[0022] In the application, the drug is vancomycin.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1) The present invention adopts a centrifugal method to classify lignin nanoparticles. By directly classifying the product (lignin nanoparticles), uniform lignin nanoparticles with a hollow structure are prepared. Compared with the traditional classification method, the present invention has the advantages of simple operation, less time consumption, high efficiency, green environmental protection, low cost, and easy industrial production;

[0025] 2) The present invention only uses a self-assembly method to load the drug - vancomycin, onto the lignin nanoparticles, and the content can be detected by HPLC, with a good release effect and a release rate of more than 80%;

[0026] 3) The present invention realizes a method for the simultaneous preparation of lignin nanoparticles and drug loading, which enables efficient drug loading and provides a new idea for the efficient use of drugs and the high-value use of lignin in the field of biomedicine. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 TEM image of crude lignin nanoparticles prepared in Example 1;

[0028] Figure 2 TEM images of crude lignin nanoparticles after centrifugal classification at different speeds in Example 2;

[0029] Figure 3 TEM structural analysis diagram of lignin nanoparticles after centrifugal classification at 1000 and 3000 rpm in Example 2; in the figure, 1000 rpm is the particle size distribution diagram of lignin nanoparticles separated at 1000 rpm; 1000 rpm-HS is the diameter distribution diagram of the hollow structure of lignin nanoparticles separated at 1000 rpm; 3000 rpm is the particle size distribution diagram of lignin nanoparticles separated at 3000 rpm; Figure, 3000 rpm-HS is the diameter distribution diagram of the hollow structure of lignin nanoparticles separated at 3000 rpm;

[0030] Figure 4 TEM structural analysis diagram of lignin nanoparticles after centrifugal classification at 5000, 8000 and 10000 rpm in Example 2; in the figure, 5000 rpm is a particle size distribution diagram of lignin nanoparticles separated at 5000 rpm; 5000 rpm-HS is a diameter distribution diagram of the hollow structure of lignin nanoparticles separated at 5000 rpm; in the figure, 8000 rpm is a particle size distribution diagram of lignin nanoparticles separated at 8000 rpm; 10000 rpm is a particle size distribution diagram of lignin nanoparticles separated at 10000 rpm;

[0031] Figure 5TEM images of purified lignin nanoparticles after centrifugal fractionation at 3000, 5000 and 8000 rpm in Example 3;

[0032] Figure 6 It is the TEM result analysis diagram of the purified lignin nanoparticles after centrifugal classification at 3000, 5000 and 8000rpm in Example 3; in the figure, KLNPs-3000 is a particle size distribution diagram of lignin nanoparticles prepared by separating and purifying lignin at a speed of 3000rpm; KLNPs-3000-HS is a diameter distribution diagram of lignin nanoparticles hollow structure prepared by separating and purifying lignin at a speed of 3000rpm; KLNPs-5000 is a particle size distribution diagram of lignin nanoparticles prepared by separating and purifying lignin at a speed of 5000rpm; KLNPs-5000-HS is a diameter distribution diagram of lignin nanoparticles hollow structure prepared by separating and purifying lignin at a speed of 5000rpm; KLNPs-8000 is a particle size distribution diagram of lignin nanoparticles prepared by separating and purifying lignin at a speed of 8000rpm; KLNPs-8000-HS is a diameter distribution diagram of lignin nanoparticles hollow structure prepared by separating and purifying lignin at a speed of 8000rpm;

[0033] Figure 7 Figure 1 is a typical image of lignin nanoparticles; in the figure, a is a side view of the hollow structure, and b is a top view of the hollow structure;

[0034] Figure 8 TEM images of lignin nanoparticle solutions at different vancomycin loadings prepared in Example 4;

[0035] Fig. 9The TEM result analysis diagram corresponding to the lignin nanoparticle solution at different vancomycin loadings prepared in Example 4; in the figure, KLNPs is a particle size distribution diagram of vancomycin-loaded lignin nanoparticles prepared with 0 mg vancomycin addition; KLNPs-HS is a diameter distribution diagram of the hollow structure of vancomycin-loaded lignin nanoparticles prepared with 0 mg vancomycin addition; VCM-KLNPs-10 is a particle size distribution diagram of vancomycin-loaded lignin nanoparticles prepared with 10 mg vancomycin addition; VCM-KLNPs-10-HS is a diameter distribution diagram of the hollow structure of vancomycin-loaded lignin nanoparticles prepared with 10 mg vancomycin addition; VCM-KLNPs-50 is a vancomycin-loaded lignin nanoparticle prepared with 50 mg vancomycin addition Particle size distribution diagram; VCM-KLNPs-50-HS is a diameter distribution diagram of the hollow structure of vancomycin-loaded lignin nanoparticles prepared with an addition of 50 mg vancomycin; VCM-KLNPs-100 is a particle size distribution diagram of vancomycin-loaded lignin nanoparticles prepared with an addition of 100 mg vancomycin; VCM-KLNPs-100-HS is a diameter distribution diagram of the hollow structure of vancomycin-loaded lignin nanoparticles prepared with an addition of 100 mg vancomycin; VCM-KLNPs-200 is a particle size distribution diagram of vancomycin-loaded lignin nanoparticles prepared with an addition of 200 mg vancomycin; VCM-KLNPs-200-HS is a diameter distribution diagram of the hollow structure of vancomycin-loaded lignin nanoparticles prepared with an addition of 200 mg vancomycin;

[0036] Fig.10 This is the elemental analysis diagram of vancomycin loaded lignin nanoparticles (VCM-KLNPs) in the TEM-mapping spectrum;

[0037] Fig.11 This is an analysis diagram of the drug loading of vancomycin loaded lignin nanoparticles. In the figure, (a) is the C18 high performance liquid chromatogram of vancomycin, (b) is the standard curve of vancomycin, (c) is the release concentration curve, and (d) is the release rate curve. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described below in conjunction with specific embodiments. In the following embodiments, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art.

[0039] The centrifuge used in the present invention is a KH20R centrifuge produced by Hunan Kaida Scientific Instrument Co., Ltd., with a centrifugal radius of 63 mm and a g of 9.8 m / s. 2 The corresponding table of the centrifuge and the speed is shown in Table 1 below:

[0040] Table 1 Correspondence between rotation speed and centrifugal force

[0041] Speed / rpm 1000 3000 5000 8000 10000 Centrifugal force / g 69 676 1741 4459 6967

[0042] The crude lignin used in the present invention is kraft lignin, which is sourced from bamboo processing residues, and the extraction and purification method adopted is the Bjorkman method.

[0043] Tetrahydrofuran, ether, dichloroethane, ethanol, and petroleum ether used in the following examples were all purchased from Nanjing Chemical Reagent Co., Ltd. and were all chemically pure. Vancomycin was purchased from Aladdin with a Cas number of 1404-90-6.

[0044] The vancomycin detection method in the following examples is as follows: high performance liquid chromatography is used, 0.05 M ammonium dihydrogen phosphate (pH = 4.0) and acetonitrile solution are used as mobile phases, eluted through a C18 chromatographic column at a flow rate of 0.8 mL / min, and the vancomycin concentration is determined under a UV detector at 220 nm.

[0045] Example 1

[0046] 20 mg of crude lignin was dissolved in 10 mL of tetrahydrofuran, and then 40 mL of distilled water was added to the tetrahydrofuran solution at a rate of 4 mL / min, and the mixed solution was stirred at a speed of 600 rpm. After centrifugation at 10000 rpm for 5 min, the precipitate was dried in a vacuum drying oven at 40°C for 48 h, and a 0.1% concentration (g / v) of lignin nanoparticle aqueous dispersion was prepared for use.

[0047] After ultrasonic treatment for 10 min, the prepared lignin nanoparticle aqueous dispersion was added dropwise to the surface of the TEM copper mesh. The surface water was evaporated under a baking lamp, and the microstructure of the lignin nanoparticles was observed using a transmission electron microscope (TEM). Figure 1 .

[0048] Figure 1 The TEM image of the microstructure of the prepared lignin nanoparticles shows that the lignin is in the form of spherical particles of varying sizes, and the surface of the large particles has an obvious hollow structure, indicating that the lignin can be prepared into lignin nanoparticles through the tetrahydrofuran / water system. However, the results also show that the preparation process is affected by many factors, and the nanometer size is extremely uneven, which can easily lead to unstable performance. Therefore, it is necessary to find a method to prepare uniform lignin nanoparticles.

[0049] Example 2

[0050] A method for efficiently preparing lignin nanoparticles with a hollow structure comprises the following steps:

[0051] 1) Dissolve 20 mg of crude lignin in 10 mL of tetrahydrofuran, then add 40 mL of distilled water to the tetrahydrofuran solution at a rate of 4 mL / min, and stir the mixed solution at a rate of 600 rpm to prepare a lignin nanoparticle suspension;

[0052] 2) The prepared lignin nanoparticle suspension was centrifuged at 1000 rpm for 5 min, and the precipitate was dried in a vacuum drying oven at 40° C. for 48 h to obtain 1000 rpm lignin nanoparticles;

[0053] 3) The supernatant after centrifugation at 1000 rpm was centrifuged at 3000 rpm for 5 min, and the precipitate was dried in a vacuum drying oven at 40° C. for 48 h to obtain 3000 rpm lignin nanoparticles;

[0054] 4) taking the supernatant after centrifugation at 3000 rpm and continuing to centrifuge at 5000 rpm for 5 min, taking the precipitate and drying it in a vacuum drying oven at 40° C. for 48 h to obtain lignin nanoparticles at 5000 rpm;

[0055] 5) The supernatant after centrifugation at 5000 rpm was centrifuged at 8000 rpm for 5 min, and the precipitate was dried in a vacuum drying oven at 40° C. for 48 h to obtain lignin nanoparticles at 8000 rpm;

[0056] 6) The supernatant after centrifugation at 8000 rpm was centrifuged at 10000 rpm for 5 min, and the precipitate was dried in a vacuum drying oven at 40° C. for 48 h to obtain lignin nanoparticles at 10000 rpm.

[0057] The dried lignin nanoparticles were prepared into a 0.1% concentration (0.1 g lignin / 100 ml water) of lignin nanoparticle aqueous dispersion and dropped onto the surface of the copper grid for TEM testing. The TEM results were analyzed using Image J software, see Table 2 and Figure 2-4 .

[0058] Table 2 Microstructure results of crude lignin nanoparticles after classification at different speeds

[0059]

[0060] From Table 2 and Figure 2-4As is known, there are more impurities in the lignin nanoparticles separated at a low speed of 1000rpm, and when the speed reaches more than 8000rpm, the hollow structures in many lignin nanoparticles disappear. According to the results of particle size, hollow diameter, etc. in Table 2, it can be found that the particle size of lignin nanoparticles as a whole decreases with the increase of separation speed, and has a good ability to classify by particle size. Through regulation, more surface area is conducive to the contact of more active groups with the outside world, which is helpful for further modification or expression of active group effects, while a smaller volume share is helpful for loading more drugs or active factors during the self-assembly process. Therefore, it has flexible applicability in the field of biomedicine.

[0061] Example 3

[0062] Dissolve 10g of crude lignin in 100mL of dichloroethane / ethanol (2:1, v / v) solution to remove surface impurities; add 1000mL of ether solution after full dissolution, stir thoroughly to precipitate lignin. Centrifuge at 8000rpm for 5min, take the precipitate, and wash the precipitate three times using 25mL of ether at 8000rpm and 5min by centrifugation. Finally, wash the precipitate once using 25mL of petroleum ether at 8000rpm and 5min by centrifugation. After fully volatilizing the surface organic solvent, vacuum dry for 12h to obtain purified lignin.

[0063] The purified lignin was prepared into a nanoparticle suspension by the anti-solvent precipitation method of Example 2, and the purified lignin nanoparticle suspension was graded by centrifugation at 3000, 5000 and 8000 rpm. In addition, the dried lignin nanoparticles were prepared into a 0.1% concentration of lignin nanoparticle aqueous dispersion and dropped onto the surface of a copper mesh for TEM testing. The TEM results were analyzed using Image J software, see Table 3 and Figure 5-6 .

[0064] Table 3 Microstructure results and surface potential of purified lignin nanoparticles after classification at different speeds

[0065] Speed / rpm 3000 5000 8000 Yield (%) 61.9 12.6 3.9 Particle size (nm) 1179±69 1052±144 836±204 Hollow structure diameter (nm) 515±112 423±126 322±128 Hollow structure surface area ratio (%) 19.2±6.1 16.0±5.2 14.3±4.7 Hollow structure volume ratio (%) 8.6±3.0 6.5±3.1 5.6±2.6 Zeta potential (mV) -24.07±1.87 -27.92±0.92 -33.51±0.32

[0066] From Table 3 and Figure 5-6It can be seen that the particle size of lignin nanoparticles decreases with the increase of rotation speed, and its particle size decreases from 1179±69nm to 836±204nm (Table 3). The size of the hollow structure of the lignin nanoparticles prepared in Example 3 also decreases with the decrease of the particle size, with more area in contact with the external environment and lower spherical mass, and has the application potential of drug delivery and gel enhancer. The lignin nanoparticles prepared after purification are stable in size and have good dispersibility, and 5000rpm is the optimal separation speed. In addition, at 8000rpm, the hollow structure of some lignin nanoparticles disappeared, indicating that this method has the ability to perform preliminary classification of lignin nanoparticles with and without hollow structures.

[0067] The crude lignin, the purified lignin prepared in Example 3, and the lignin nanoparticles obtained at centrifugal speeds of 3000, 5000, and 8000 rpm were centrifuged by 600M nuclear magnetic resonance. 31 P was used to detect the functional group content, see Table 4.

[0068] Table 4 Functional group content of lignin nanoparticles at different rotation speeds

[0069]

[0070] Figure 7 It is a typical lignin nanoparticle diagram; in the figure, a is a side view of the hollow structure, and b is a top view of the hollow structure. It can be found that lignin has an obvious hollow structure, and the lignin wall is thicker at the end away from the hollow structure. The side confirms that it forms lignin nanoparticles through layer-by-layer self-assembly stacking. As shown in Table 4, lignin has a higher hydrophilic group-total phenolic hydroxyl and carboxyl content at high speed. Therefore, it is speculated that this may be due to the fact that more hydrophilic groups cause the formation of lignin nanoparticles to slow down. With the increase of the anti-solvent (water) content, the concentration difference between the inside and outside gradually decreases, the lignin wall is insufficiently formed, and the collapse leads to a decrease in particle size, and even the disappearance of the hollow structure. It has the ability to adjust the size of the hollow structure of nanoparticles by regulating the hydrophilic and hydrophobic ratio in the reaction system.

[0071] Example 4

[0072] 100 mg of the purified lignin prepared in Example 3 and 0 mg, 10 mg, 50 mg, 100 mg, and 200 mg of vancomycin were dissolved in 50 mL of tetrahydrofuran, and 200 mL of aqueous solution was added dropwise at a speed of 4 mL / min to prepare drug-loaded lignin nanoparticles (VCM-KLNPs-10, VCM-KLNPs-50, VCM-KLNPs-100, and VCM-KLNPs-200). After centrifugation at 5000 rpm for 5 min, the precipitate was placed in a vacuum drying oven and dried for 48 h, and prepared into a 0.1% concentration of drug-loaded lignin nanoparticle aqueous dispersion. After ultrasonication for 10 min, it was added dropwise to the surface of a TEM-specific copper mesh, and the surface water was evaporated under a baking lamp. The microstructure of the lignin nanoparticles was observed using a transmission electron microscope (TEM), as shown in Table 5 and Figure 8-9 .

[0073] Table 5 Microstructure and surface potential analysis of lignin nanoparticle solutions at different vancomycin loadings

[0074]

[0075] From Table 5 and Figure 8-9 It can be seen that the loading amount of vancomycin has little effect on the size of lignin nanoparticles, which is about 1000 nm, but the size of its hollow structure increases with the increase of the content of the added hydrophobic drug vancomycin. The result is consistent with the speculation obtained in Example 3: more hydrophilic groups lead to slower formation of lignin nanoparticles. With the increase of the anti-solvent (water) content, the concentration difference between the inside and the outside gradually decreases, the lignin wall is insufficiently formed, and the collapse leads to a decrease in particle size, and even the disappearance of the hollow structure. It has the ability to adjust the size of the hollow structure of nanoparticles by regulating the hydrophilic-hydrophobic ratio in the reaction system.

[0076] The vancomycin concentration detection method was constructed by C18-HPLC, and the surface element distribution was analyzed by scanning in mapping mode. The prepared VCM-KLNPs-10, VCM-KLNPs-50, VCM-KLNPs-100, and VCM-KLNPs-200 were subjected to vancomycin drug sustained release assay. The results are shown in Fig.10 and Fig.11 .

[0077] The specific steps of the vancomycin concentration detection method are as follows:

[0078] 1) Weigh 12 mg of vancomycin-loaded lignin nanoparticles, add 6 mL of 0.01 M PBS solution to make a 2 mg / mL suspension, and sonicate for 10-30 min;

[0079] 2) Take 5 mL of the suspension prepared in step 1) into a dialysis bag, put it into 100 mL of PBS solution and dialyze at 100 rpm, and take samples at 0.5, 1, 2, 4, 8, 12, 24, 48, 72 and 96 h. Take 3 mL of liquid each time during the sampling process, and add 3 mL of PBS solution. Centrifuge the samples at each time point at 10,000 rpm for 5 min, filter with a 0.22 μm filter membrane, and prepare HPLC samples; the measured content is used to draw the sustained-release curve of vancomycin.

[0080] 3) Take another 1 mL of the suspension prepared in step 1) and centrifuge at 10000 rpm for 5 min, filter through a 0.22 μm filter membrane, and prepare an HPLC sample. The measured content is used to calculate the drug loading rate of vancomycin.

[0081]

[0082] Among them, M VCM is the mass of vancomycin in the suspension prepared in step 1), g; M VCM-LNPs The mass of vancomycin-loaded lignin nanoparticles in the suspension prepared in step 1), g.

[0083] Table 6 Surface element distribution and drug loading rate of lignin nanoparticles at different vancomycin loadings

[0084]

[0085]

[0086] From Table 6 and Fig.10 It can be seen that the distribution of Cl element was successfully determined, indicating that vancomycin was successfully loaded onto the lignin nanoparticles, and the lignin nanoparticles with a vancomycin loading of 100 mg had the highest detection rate of vancomycin and had a good loading capacity.

[0087] Depend on Fig.11 It can be seen that the chromatographic system constructed by the present invention has good detection performance. At the same time, vancomycin loaded lignin nanoparticles have a good sustained release effect, and the sustained release rate is greater than 80%. It shows the most suitable loading effect at a loading amount of 100 mg, and the drug loading rate is 6.45%, indicating that the lignin nanoparticles prepared by this method have good drug delivery ability.

[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for efficiently preparing lignin nanoparticles with a hollow structure, characterized in that: A lignin nanoparticle suspension is prepared by an anti-solvent precipitation method using a tetrahydrofuran-water system, and uniform lignin nanoparticles with a hollow structure are obtained by controlling the rotation speed for classification; wherein the hollow structure diameter of the uniform lignin nanoparticles with a hollow structure is 423-715 nm, and the hollow structure surface area accounts for 19.98-34.3%.

2. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 1, characterized in that: The lignin is amphiphilic lignin.

3. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 1, characterized in that: The controlled rotation speed classification is to classify the lignin nanoparticles with hollow structures and those without hollow structures at a rotation speed of 5000 rpm.

4. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 1, characterized in that: The lignin nanoparticle suspension is prepared directly by using an anti-solvent precipitation method of a tetrahydrofuran-water system without prior classification treatment, wherein the tetrahydrofuran is a solvent and the aqueous solution is an anti-solvent.

5. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 1, characterized in that: The following steps are involved: 1) dissolving lignin in tetrahydrofuran, and then adding dropwise the aqueous solution and stirring to obtain a lignin nanoparticle suspension; 2) centrifuging the prepared lignin nanoparticle suspension at a rotation speed of 1000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain 1000 rpm lignin nanoparticles; 3) taking the supernatant after centrifugation at 1000 rpm and continuing to centrifuge at 3000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 3000 rpm; 4) taking the supernatant after centrifugation at 3000 rpm and continuing to centrifuge at 5000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 5000 rpm; 5) taking the supernatant after centrifugation at 5000 rpm and continuing to centrifuge at 8000 rpm, taking the precipitate and drying it in a vacuum drying oven to obtain lignin nanoparticles at 8000 rpm; 6) The supernatant after centrifugation at 8000 rpm is centrifuged again at 10000 rpm, and the precipitate is dried in a vacuum drying oven to obtain lignin nanoparticles at 10000 rpm.

6. The method for efficiently preparing lignin nanoparticles with a hollow structure according to claim 5, characterized in that: The centrifugation time is 5 minutes, and the drying temperature in the vacuum drying oven is 40°C.

7. The method for efficiently preparing lignin nanoparticles with a hollow structure according to any one of claims 1 to 6, wherein the lignin nanoparticles with a hollow structure are prepared.

8. Use of the lignin nanoparticles with a hollow structure according to claim 7 in drug loading.

9. The use according to claim 8, characterized in that: Lignin and drugs are added into tetrahydrofuran at the same time, and then an aqueous solution is added dropwise to obtain a mixed suspension, and the mixed suspension is centrifuged to obtain drug-loaded lignin nanoparticles.

10. The use according to claim 9, characterized in that: The drug is vancomycin.