Preparation method of composite reinforced polyolefin-based film and composite reinforced polyolefin-based film

By growing silica particles on the surface of the polyolefin film and wrapping a cellulose thickener to form a composite layer, the problem of poor wettability of the polyolefin film is solved, and firm hydrophilic modification and improvement of film performance are achieved.

CN118185100BActive Publication Date: 2024-11-12GUANGDONG GUNNER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410466064.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-11-12
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

Polyolefin films are limited by poor wetting due to their low surface energy in filter membranes and battery separators applications. Existing modification methods such as graft modification and coating modification have material integrity damage and high cost. Uneven layer thickness and shedding problems.

Method used

Polyolefin films are prepared by bidirectional stretching method, and silica particles are grown on its surface by in-situ polymerization, and silica particles are wrapped with cellulose thickener to form a cellulose-silica composite layer to enhance the film Hydrophilicity and adhesion.

Benefits of technology

The hydrophilicity of the polyolefin film is significantly improved, and the adhesive properties of the cellulose layer make the silica particles firmly adhere to avoid falling off. It is simple to operate, low cost, and has little impact on the air permeability and thickness uniformity of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118185100B_ABST
    Figure CN118185100B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method of a composite reinforced polyolefin-based film and a composite reinforced polyolefin-based film. First, a biaxially oriented polyolefin film is prepared, and the film is immersed in a specially configured precursor solvent and shaken to fully react. The film after the reaction is rinsed with distilled water and then dried to obtain a monodisperse silica-enhanced polyolefin film, and then the surface of the monodisperse silica-enhanced polyolefin film is glued to a cellulose layer by, for example, vacuum filtration / pressure difference method / immersion method, and finally the film is annealed to finally obtain a cellulose-silicon dioxide composite reinforced polyolefin-based film. The composite reinforced polyolefin-based film prepared by the present invention has a dual hydrophilic effect produced by the combination of cellulose and silica, so that the hydrophilicity of the polyolefin film surface is significantly improved, and the hydrophilic modified layer can be firmly adhered to the film surface and is not easy to fall off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new materials, and in particular to a preparation method of a composite reinforced polyolefin-based film and the composite reinforced polyolefin-based film. Background Art

[0002] Polyolefin films are widely used due to their good mechanical properties, good chemical stability, excellent electrochemical properties, low price, etc. However, due to their low surface energy, their wettability is poor, which limits their application in the fields of filtration membranes and battery separators.

[0003] To address this defect, there are currently many methods for hydrophilic modification of polyolefin films, including grafting modification, coating modification, etc. Grafting modification is to graft some hydrophilic groups on the surface of polyolefin films. Commonly used grafting methods include ultraviolet radiation, electron beam radiation, plasma radiation, etc. These methods will damage the integrity of the film material to a certain extent, and the modification methods are complex and costly. The coating modification method can quickly compound the hydrophilic material and the polyolefin film, but the coating layer and the film surface are physically adhered, and there is a problem of loose contact between the contact layers; and the coating layer is generally thicker (>2μm), which affects the film thickness, air permeability and other properties; furthermore, the coating layer will form larger particles due to the agglomeration effect, which affects the uniformity of the film thickness.

[0004] Therefore, a method is needed to hydrophilically modify the surface of a polyolefin film and ensure that the hydrophilic modified layer can firmly adhere to the surface of the film without falling off. Summary of the invention

[0005] The embodiments of the present invention provide a method for preparing a composite reinforced polyolefin-based film and a composite reinforced polyolefin-based film to at least solve one of the problems existing in the related art. To achieve this purpose, the present invention is implemented by the following technical solutions.

[0006] One aspect of the present invention provides a method for preparing a composite reinforced polyolefin-based film, comprising:

[0007] Step 1: preparing a polyolefin-based film by a biaxial stretching method;

[0008] Step 2: Mix 1-10 parts of tannic acid with 100-1000 parts of buffer solution to obtain solution 1;

[0009] Step 3: adding 1-10 parts of 3-aminopropylsilicon dioxide-based triethoxysilane and 1-10 parts of tetraethyl orthosilicate to 100-1000 parts of at least one of alcohols, phenols and ketones to obtain a solution 2;

[0010] Step 4: Mix solution 1 and solution 2 to obtain solution 3;

[0011] Step 5: immersing the polyolefin-based film obtained in step 1 in solution 3, allowing silica particles to grow uniformly inside and on the surface of the polyolefin-based film through in-situ polymerization, and obtaining a monodisperse silica-reinforced polyolefin film after washing and drying;

[0012] Step 6: dissolving 0.05-0.2% by mass of a cellulose thickener in distilled water to obtain a cellulose aqueous solution;

[0013] Step 7: The cellulose aqueous solution is allowed to interact with the monodisperse silica-reinforced polyolefin film, and after annealing, a cellulose-silica composite reinforced polyolefin-based film is obtained, wherein the cellulose thickener wraps the silica particles attached to the surface of the polyolefin-based film.

[0014] Furthermore, the pH value of the buffer solution is 6 to 8.5.

[0015] Furthermore, step 5 further includes: immersing the polyolefin-based film obtained in step 1 in solution three, shaking to allow sufficient reaction, allowing silica particles to grow evenly inside and on the surface of the polyolefin-based film through in-situ polymerization, and obtaining a monodisperse silica-reinforced polyolefin film after cleaning and drying.

[0016] Furthermore, step 7 further comprises: interacting the cellulose aqueous solution with the monodisperse silica reinforced polyolefin film by vacuum filtration method, pressure difference method or immersion method, so that the cellulose thickener is adhered to the surface of the monodisperse silica reinforced polyolefin film, and after annealing treatment, a cellulose-silica composite reinforced polyolefin-based film is obtained, wherein the cellulose thickener wraps the silica particles attached to the surface of the polyolefin-based film.

[0017] Furthermore, step 1 includes: adding at least one polyolefin-based polymer and a lubricant into a twin-screw extruder, blending and extruding a gel film, and then stretching the gel film into a film through a biaxial stretching process, and obtaining a polyolefin-based film through extraction and annealing.

[0018] Further, the thickness of the polyolefin-based film is not more than 5 μm.

[0019] Furthermore, the particle size of the silicon dioxide particles dispersed inside and on the surface of the polyolefin-based film is 5-100 nm, and the thickness of the silicon dioxide attached to the surface of the polyolefin-based film is not more than 1 μm.

[0020] Furthermore, the mixing temperature in step 2 is 70-90° C., and the mixing time is 5-20 min; the mixing temperature in step 3 is 0-100° C., and the mixing time is 5-20 min.

[0021] Furthermore, the mixing temperature in step 4 is 70-90° C., and the mixing time is 5-20 min.

[0022] On the other hand, the present invention provides a composite reinforced polyolefin-based film prepared according to the preparation method of the above-mentioned composite reinforced polyolefin-based film, wherein the composite reinforced polyolefin-based film is a cellulose-silicon dioxide composite reinforced polyolefin-based film, wherein the silicon dioxide particles are uniformly grown inside and on the surface of the polyolefin-based film, and the cellulose thickener wraps the silicon dioxide particles attached to the surface of the polyolefin-based film.

[0023] The embodiments of the present invention have the following beneficial effects:

[0024] (1) Silicon dioxide (SiO 2 ) has a large specific surface area and is easy to produce a large number of silanol groups (Si-OH), so it has an excellent effect as a filler for improving the hydrophilicity of polyolefin films. The present invention grows silica nano-ceramic particles inside and on the surface of the polyolefin film by in-situ polymerization, which can be well bonded to the polyolefin film; further, a cellulose thickener is used to wrap the silica inorganic particles attached to the surface of the film. Due to the strong bonding force between cellulose and the polyolefin film, the silica inorganic filler can be more firmly attached to the surface of the film through the cellulose layer, thereby effectively avoiding the inorganic particles from falling off the surface of the polyolefin-based film during use.

[0025] (2) At the same time, the surface of cellulose molecules carries a large number of hydroxyl (-OH) functional groups, which can form hydrogen bonds with water molecules, showing strong hydrophilicity. The dual hydrophilic effect produced by the combination of cellulose and silica significantly improves the hydrophilicity of the polyolefin film surface, and the hydrophilic modified layer can firmly adhere to the film surface and is not easy to fall off.

[0026] (3) Compared with chemical modification and irradiation treatment of the polyolefin-based surface, the present invention prepares a monodisperse silica-reinforced polyolefin film by a sol-gel method, and then adheres the cellulose layer by methods such as vacuum filtration / pressure difference method / immersion method, and finally anneals to obtain a cellulose-silica composite reinforced polyolefin-based film material. The preparation method provided by the embodiment of the present invention has simple operation steps, and the cellulose adhesive is low in cost and has bio-environmental friendliness.

[0027] (4) The thickness of the silica inorganic filler layer prepared according to the embodiment of the present invention is thin, not exceeding 1 μm, and thus has little effect on other properties of the entire film (including thickness, air permeability, etc.).

[0028] (5) The silica filler particles are evenly dispersed inside and on the surface of the polyolefin film with a smaller radius, improving the uniformity of the overall thickness of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0030] Figure 1 The diagram is a schematic diagram of the interface contact angle and membrane water flux changes under different ratios of cellulose and silane in the embodiment of the present invention. The broken line in the figure represents the change of water flux, and the bar graph represents the change of the solid-liquid contact angle on the surface of the modified membrane;

[0031] Figure 2 The solid-liquid contact images of the interface of the composite reinforced polyolefin-based film of the embodiment of the present invention when the ratios of hydroxyethyl cellulose to 3-aminopropylsilicon dioxide-based triethoxysilane are 1:0, 1:1, 1:2, and 1:3 respectively;

[0032] Figure 3 This is a SEM (scanning electron microscope) image of the surface of the polyolefin-based film of Comparative Example 2 of Example 1 of the present invention, and the upper right corner of the image is an image of the solid-liquid interface contact on the film surface;

[0033] Figure 4 This is a SEM image of the surface of a single-phase silica-reinforced polyolefin-based film of Comparative Example 1 of Example 1 of the present invention, and the upper right corner of the image is an image of the solid-liquid interface contact on the surface of the single-phase silica-reinforced polyolefin-based film;

[0034] Figure 5 This is a SEM image of the surface of the cellulose-silicon dioxide composite reinforced polyolefin-based film of Example 1 of the present invention, and the upper right corner of the image is an image of the solid-liquid interface contact on the surface of the cellulose-silicon dioxide composite reinforced film;

[0035] Figure 6 A line graph showing the relationship between the mixing reaction time and water flux in the silane solvent preparation for 0.2 g of cellulose and a film thickness of 700 nm (solid film 367 nm). DETAILED DESCRIPTION

[0036] To make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. However, it will be appreciated by those skilled in the art that in the embodiments of the present invention, many technical details are proposed in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical scheme claimed in the present application can be implemented. The division of the following embodiments is for the convenience of description, and should not constitute any limitation on the specific implementation of the present invention. The various embodiments can be combined and referenced with each other without contradiction.

[0037] The embodiment of the present invention provides a method for preparing a composite reinforced polyolefin-based film. First, a biaxially oriented polyolefin film is prepared, and the film is immersed in a specially configured precursor solvent and shaken to allow it to react fully. The film after the reaction is rinsed with distilled water and then dried to obtain a monodisperse silica-reinforced polyolefin film, and then a cellulose layer is glued to the surface of the monodisperse silica-reinforced polyolefin film by, for example, vacuum filtration / pressure difference method / immersion method, and finally the film is annealed to finally obtain a cellulose-silica composite reinforced polyolefin-based film. The specific method is as follows:

[0038] Step 1: Prepare a polyolefin-based film by biaxial stretching. Specifically, one or two polyolefin-based polymers and a lubricant are added to a twin-screw extruder, co-extruded into a gel film, and then stretched into an ultra-thin film by a biaxial stretching process, and finally processed by extraction, annealing, etc. to prepare a polyolefin-based film. The thickness of the polyolefin-based film is not more than 5 μm.

[0039] Step 2: Mix 1-10 parts of tannic acid with 100-1000 parts of Tris-hydrochloric acid buffer to obtain solution 1. The pH value of the Tris-hydrochloric acid buffer is 6-8.5, the mixing temperature is 70-90° C., and the mixing time is 5-20 minutes.

[0040] Step 3: 1-10 parts of 3-aminopropylsilicon dioxide triethoxysilane and 1-10 parts of tetraethyl orthosilicate are added to 100-1000 parts of at least one of alcohols, phenols and ketones (such as methanol, ethanol and propanol) to obtain solution 2. The mixing temperature is 0-100° C. and the mixing time is 5-20 minutes.

[0041] Step 4: Mix solution 1 and solution 2 to obtain solution 3. The mixing temperature is 70-90° C. and the mixing time is 5-20 min.

[0042] Step 5: Immerse the polyolefin-based film obtained in step 1 in solution three, shake it to fully react, and make the silica particles grow evenly inside and on the surface of the polyolefin-based film through in-situ polymerization. After cleaning and drying, a monodisperse silica-enhanced polyolefin film is obtained. Among them, the particle size of the silica particles dispersed inside and on the surface of the polyolefin-based film does not exceed 1 μm, and in this embodiment, it is 5-100nm. The silica filler particles are evenly dispersed inside and on the surface of the polyolefin film with a smaller radius, which improves the uniformity of the overall thickness of the film. The thickness of the silica attached to the surface of the polyolefin-based film is no more than 1 μm. Since the thickness of the silica inorganic filler layer is thin, it has little effect on other properties of the film as a whole (including thickness, air permeability, etc.).

[0043] Step 6: Dissolve 0.05-0.2% of cellulose thickener in distilled water to obtain a cellulose aqueous solution.

[0044] Step 7: The cellulose aqueous solution and the monodisperse silica reinforced polyolefin film are interacted by, for example, vacuum filtration, pressure difference or immersion, so that the cellulose thickener adheres to the surface of the monodisperse silica reinforced polyolefin film, and then the film is placed in an oven at 100-130°C for drying for 10-60 minutes for annealing treatment to obtain a cellulose-silica composite reinforced polyolefin-based film, wherein the cellulose thickener wraps the silica particles attached to the surface of the polyolefin-based film.

[0045] The implementation effects of the present invention are further demonstrated below through specific embodiments.

[0046] Embodiment 1:

[0047] Step (1): adding ultra-high molecular weight polyethylene and petrolatum in a ratio of 9:1 into a twin-screw extruder, blending and extruding a gel film, and then stretching it into an ultra-thin film through a biaxial stretching process, and finally preparing a polyolefin-based film through extraction, annealing and other treatments. The aspect ratio of the twin-screw extruder is 11:1, the screw speed of the extruder is 200 rpm, and the temperature of each zone of the extruder is 150-200°C.

[0048] Step (2): Mix 0.5 g of tannic acid with 50 ml of Tris-HCl buffer (pH 8.5) in proportion.

[0049] Step (3): Add 0.5 g of 3-aminopropyltriethoxysilane and 0.2 ml of tetraethyl orthosilicate and 10-100 ml of ethanol and mix according to the proportion.

[0050] Step (4): Mix the solvents prepared in step (2) and step (3).

[0051] Step (5): The polyolefin film prepared in step (1) is immersed in the solvent obtained in step (4), and shaken for 1 hour to allow the reaction to proceed fully.

[0052] Step (6): The film treated in step (5) is rinsed with distilled water and then placed in an oven at 100° C. to dry for 2 hours, thereby preparing a monodisperse silica reinforced polyolefin film.

[0053] Step (7): fully dissolving 0.1 wt % (mass percentage) of hydroxyethyl cellulose in distilled water to obtain a hydroxyethyl cellulose aqueous solution.

[0054] Step (8): Place the monodisperse silica-reinforced polyolefin film obtained in step (6) in a vacuum filtration device. Adhere the hydroxyethyl cellulose aqueous solution obtained in step (7) to the film obtained in step (6) by vacuum filtration to obtain a cellulose / silicon dioxide composite reinforced polyolefin-based film. Finally, place the film in an oven at 125°C and dry for 30 minutes for annealing. The solution loading rate at the inlet of the filtration device is set to 5 ml / cm based on the film size. 2 .

[0055] Comparative Example 1:

[0056] The difference between this comparative example and Example 1 is that the treatment processes of step (7) and step (8) are not performed. That is, a single-phase silica-reinforced polyolefin-based film is prepared.

[0057] Comparative Example 2:

[0058] The difference between this comparative example and Example 1 is that only step (1) is performed, that is, a polyolefin-based film is prepared.

[0059] The wettability of the single-phase silica-reinforced polyolefin-based film and the polyolefin-based film prepared in Example 1, Comparative Example 1 and Comparative Example 2 was tested, and the surface of the material was imaged by scanning electron microscope (SEM). The test and imaging results are shown in FIG. Figure 3-Figure 5 It can be seen that the addition of cellulose thickener can effectively avoid the phenomenon of inorganic nanoparticles falling off from the surface of polyolefin materials without changing the excellent performance of silica inorganic nanoparticles in enhancing polyolefin-based films, thereby enhancing the effect of silica on improving the hydrophilicity of polyolefin-based films.

[0060] Embodiment 2:

[0061] The difference between this embodiment and embodiment 1 is that the cellulose thickener in step (7) is hydroxymethyl cellulose.

[0062] Embodiment 3:

[0063] The difference between this embodiment and embodiment 1 is that the lubricant in step (1) is polyethylene wax.

[0064] Embodiment 4:

[0065] The difference between this embodiment and embodiment 1 is that the cellulose in step (7) is carboxymethyl cellulose.

[0066] Embodiment 5:

[0067] The difference between this embodiment and embodiment 1 is that in step (1), the polyolefin material is polypropylene, the lubricant is polypropylene wax, and the temperature of each zone of the extruder is 170-220°C.

[0068] Embodiment 6:

[0069] The difference between this embodiment and embodiment 1 is that in step (1), the polyolefin material is high-density polyethylene, the lubricant is polyethylene wax, and the temperature of each zone of the extruder is 150-190°C.

[0070] Embodiment 7:

[0071] The difference between this embodiment and embodiment 1 is that the cellulose used in step (7) is hydroxypropyl cellulose.

[0072] Embodiment 8:

[0073] The difference between this embodiment and embodiment 1 is that in step (1), the polyolefin material is low-density polyethylene, the lubricant is polyethylene wax, and the temperature of each zone of the extruder is 150-190°C.

[0074] Embodiment 9:

[0075] The difference between this embodiment and embodiment 1 is that in step (1), the polyolefin material is polyethylene, the lubricant is polyethylene wax, and the temperature of each zone of the extruder is 150-190°C.

[0076] Example 10: The difference between this example and Example 1 is that the mass ratio of the silane added in step (3) to the cellulose added in step (7) is 0:1, 1:1, 2:1, and 3:1 respectively. Finally, the obtained samples are tested and analyzed.

[0077] The water flux and surface hydrophilicity of the polyolefin-based films modified with different filler ratios were tested. The test results are shown in Figure 1 , Figure 2 shown. Figure 1 It is a schematic diagram of the change of the interface contact angle and the membrane water flux under different ratios of cellulose and silane according to an embodiment of the present invention. Figure 2 The solid-liquid contact images of the composite reinforced polyolefin-based film interface when the ratio of cellulose (HEC) to silane is 1:0, 1:1, 1:2, and 1:3, respectively. It can be seen from the figure that different ratios between modified fillers can produce different effects on the hydrophilicity of the material surface and the wettability of the material. When the ratio of cellulose (HEC) to silane is 1:3, the film hydrophilicity modification effect is the best, the contact angle is 0°, and it is completely wetted.

[0078] Example 11: The difference between this example and Example 1 is that the mixing time in step (3) is 1min, 2mi, 3min, 5min, and 10min for different samples, and finally the obtained samples are tested and analyzed. The water flux test of the modified polyolefin-based films obtained with different mixing times is performed, and the test results are shown in Figure 6 It can be seen from the figure that the mixing time of the silane solvent preparation can have different effects on the wettability of the material. When the mixing time of step (3) is 5 minutes, the obtained modified polyolefin-based film has the largest flux and the best hydrophilic modification effect.

[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a composite reinforced polyolefin-based film, characterized in that: include: Step 1: preparing a polyolefin-based film by a biaxial stretching method; Step 2: Mix 1-10 parts of tannic acid with 100-1000 parts of buffer solution to obtain solution 1; Step 3: adding 1-10 parts of 3-aminopropylsilicon dioxide-based triethoxysilane and 1-10 parts of tetraethyl orthosilicate to 100-1000 parts of at least one of alcohols, phenols and ketones to obtain a solution 2; Step 4: Mix solution 1 and solution 2 to obtain solution 3; Step 5: immersing the polyolefin-based film obtained in step 1 in solution 3, allowing silica particles to grow uniformly inside and on the surface of the polyolefin-based film through in-situ polymerization, and obtaining a monodisperse silica-reinforced polyolefin film after washing and drying; Step 6: dissolving 0.05-0.2% by mass of a cellulose thickener in distilled water to obtain a cellulose aqueous solution; Step 7: The cellulose aqueous solution is allowed to interact with the monodisperse silica-reinforced polyolefin film, and after annealing, a cellulose-silica composite reinforced polyolefin-based film is obtained, wherein the cellulose thickener wraps the silica particles attached to the surface of the polyolefin-based film.

2. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: The pH value of the buffer solution is 6-8.

5.

3. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: Step 5 further includes: immersing the polyolefin-based film obtained in step 1 in solution 3, shaking to allow sufficient reaction, allowing silica particles to grow evenly inside and on the surface of the polyolefin-based film through in-situ polymerization, and obtaining a monodisperse silica-reinforced polyolefin film after cleaning and drying.

4. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: Step 7 further comprises: interacting the cellulose aqueous solution with the monodisperse silica reinforced polyolefin film by vacuum filtration, pressure difference or immersion, so that the cellulose thickener adheres to the surface of the monodisperse silica reinforced polyolefin film, and after annealing, obtaining a cellulose-silica composite reinforced polyolefin-based film, wherein the cellulose thickener wraps the silica particles attached to the surface of the polyolefin-based film.

5. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: Step 1 comprises: adding at least one polyolefin-based polymer and a lubricant into a twin-screw extruder, blending and extruding a gel film, and then stretching the gel film into a film through a biaxial stretching process, and obtaining a polyolefin-based film through extraction and annealing treatment.

6. The method for preparing a composite reinforced polyolefin-based film according to claim 5, characterized in that: The thickness of the polyolefin-based film is not more than 5 μm.

7. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: The particle size of the silicon dioxide particles dispersed inside and on the surface of the polyolefin-based film is 5-100 nm, and the thickness of the silicon dioxide attached to the surface of the polyolefin-based film is not more than 1 μm.

8. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: The mixing temperature in step 2 is 70-90° C., and the mixing time is 5-20 min; the mixing temperature in step 3 is 0-100° C., and the mixing time is 5-20 min.

9. The method for preparing a composite reinforced polyolefin-based film according to claim 1, characterized in that: The mixing temperature in step 4 is 70-90° C., and the mixing time is 5-20 min.

10. A composite reinforced polyolefin-based film prepared according to the method for preparing a composite reinforced polyolefin-based film according to any one of claims 1 to 9, characterized in that: The composite reinforced polyolefin-based film is a cellulose-silicon dioxide composite reinforced polyolefin-based film, wherein silicon dioxide particles are uniformly grown inside and on the surface of the polyolefin-based film, and the cellulose thickener wraps the silicon dioxide particles attached to the surface of the polyolefin-based film.