Iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution and preparation method and application thereof
By regulating the particle size and crystal surface exposure of the iridium oxygen composite, an iridium oxygen nanocatalyst for electrocatalytic oxygen evolution was prepared, which solved the instability of the iridium oxygen composite in the electrocatalytic reaction, and improved the catalytic activity and Industrial production efficiency.
Patent Information
- Application Number
- CN202410432854.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-11
AI Technical Summary
The existing iridium oxygen composite catalysts have the valence ratio, particle size and instability of the exposed crystal surface in the electrocatalytic oxygen evolution reaction, which affects its catalytic activity and industrial production efficiency.
By adding organic ligands to chloroiritic acid and adjusting pH, vacuum freeze-drying and calcining treatment, controlling the particle size and crystal surface exposure of the iridium oxygen composite, an iridium oxygen nanocatalyst with a specific crystal surface structure was prepared.
It significantly reduces the overpotential, increases the current density, improves the stability and performance of the catalyst, simplifies the preparation process, and reduces production costs.
Smart Images

Figure CN118186482B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material synthesis and electrocatalysis, and in particular to an iridium oxygen composite nano catalyst for electrocatalytic oxygen evolution, and a preparation method and application thereof. Background Art
[0002] Currently, more than 80% of the world's energy demand is met by burning fossil fuels such as oil or natural gas. However, due to the accelerated consumption of fossil fuels and the resulting environmental pollution, advanced sustainable energy storage and conversion technologies have attracted widespread attention from academia and industry. Therefore, the zero-carbon emission splitting of water into hydrogen and oxygen to store energy into chemical fuels is seen as an environmentally friendly option and widely regarded as a key step to address the rapid growth of energy consumption and related environmental issues. Proton exchange membrane water electrolysis (PEMWE) provides a promising route to produce green hydrogen from renewable energy and may become a master key to unlock future sustainable energy systems. As the bottleneck half-reaction of water splitting, the oxygen evolution reaction (OER) needs to overcome its sluggish kinetics due to its excessive overpotential for the four-electron and four-proton transfer process at the anode. Currently, iridium-based oxides are still considered the only viable option for practical applications due to their high activity and considerable corrosion stability under harsh electrochemical reaction conditions. To improve the overall efficiency of PEMWE, future electrocatalyst development strategies must simultaneously address performance indicators in terms of activity, stability, and material cost. To improve the utilization of iridium, efforts have been directed toward increasing the electrochemical surface area of the catalyst per unit mass of iridium, thereby increasing the number of available electrocatalytic surface active sites.
[0003] Electrolysis of water into clean and renewable hydrogen in acidic electrolytes is an effective technology to alleviate energy and environmental protection issues. Effective electrocatalysts for anodic oxygen evolution reaction significantly improve the energy conversion efficiency because most of the energy consumption of electrolytic water splitting occurs at the anode. Iridium oxide (IrO2) is considered to be a state-of-the-art OER catalyst that can withstand harsh acidic conditions. However, previously reported IrO2 catalysts lack high intrinsic activity due to the sluggish kinetics of OER.
[0004] In the Chinese patent with application number 202111118902.1, a composite catalyst of iridium and iridium oxide was mainly synthesized, but the characteristic peak of iridium oxide did not appear. In the Chinese patent with application number 202210069738.8, an Ir@IrOx core-shell catalyst was mainly synthesized, but its process was complicated and required the introduction of inert gas, which is not conducive to large-scale industrial production.
[0005] The technology of using the reducing power of the ligand itself to regulate the valence ratio of the iridium element in the iridium-oxygen complex and changing the calcination temperature and time to control the particle size and exposed crystal surface of the generated iridium-oxygen complex has not been reported yet. Summary of the invention
[0006] Based on the prior art, the present invention designs and develops an iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution. One of the inventive objectives of the present invention is to solve the problem of the valence ratio of iridium element in the iridium-oxygen composite.
[0007] The second purpose of the present invention is to solve the problem of particle size and exposed crystal surface of iridium-oxygen complex.
[0008] The present invention designs and develops a method for preparing an iridium-oxygen complex nanocatalyst for electrocatalytic oxygen evolution. The purpose of the present invention is to solve the problem of regulating the valence ratio of the iridium element in the iridium-oxygen complex by the reducing strength of the ligand itself, and to control the particle size and exposed crystal surface of the generated iridium-oxygen complex by changing the calcination temperature and time.
[0009] The present invention also designs and develops an application of an iridium-oxygen composite nanocatalyst in anode electrocatalytic oxygen evolution.
[0010] The technical solution provided by the present invention is:
[0011] An iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution, comprising: an XRD spectrum of the iridium-oxygen composite nanocatalyst including a (101) crystal plane diffraction peak of IrO2 and no (110) crystal plane diffraction peak; and
[0012] It includes the (311) crystal plane diffraction peak and (222) crystal plane diffraction peak of Ir, but there is no (211) crystal plane diffraction peak.
[0013] Preferably, the particle size of the iridium-oxygen composite nanocatalyst is 2 to 5 nm.
[0014] Preferably, the iridium-oxygen composite nanocatalyst has a surface that exposes a (111) crystal plane.
[0015] A method for preparing an iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution comprises the following steps:
[0016] Step 1, adding an organic ligand to chloroiridic acid, stirring continuously, and adjusting the pH to react;
[0017] Step 2: After the reaction is completed, vacuum freeze-drying is performed to obtain a precursor;
[0018] Step three: calcining the precursor and washing it to obtain the iridium-oxygen composite nanocatalyst.
[0019] Preferably, in step 1, the organic ligand is L-aspartic acid, oxalic acid or succinic acid.
[0020] Preferably, in the step 1, the amount of the organic ligand added is 0.2 g to 0.8 g.
[0021] Preferably, in the step 1, the amount of chloroiridic acid added is 0.1 g to 0.3 g.
[0022] Preferably, in step 1, the pH is adjusted to 2-11.
[0023] Preferably, in the step three, the calcination conditions include: the calcination temperature range is 300° C. to 700° C., and the calcination time range is 10 to 60 min.
[0024] The iridium-oxygen composite nanocatalyst is used in the electrocatalytic oxygen evolution at the anode.
[0025] The beneficial effects of the present invention are:
[0026] 1. The present invention uses iridium-oxygen composite nanocatalyst as an anode catalyst for electrocatalytic oxygen evolution, which has the effect of significantly reducing overpotential and increasing current;
[0027] 2. The synthesis method of the iridium-oxygen composite nanocatalyst provided by the present invention is simple and time-saving. The obtained nanoparticles have uniform size, stable performance, and significant effect in promoting oxygen evolution.
[0028] 3. The preparation method of the iridium-oxygen composite nanocatalyst of the present invention is simple and convenient, does not require expensive instruments and equipment, is easy to operate, economical and environmentally friendly;
[0029] 4. The iridium-oxygen composite nanocatalyst prepared by the invention has stable performance, uniform size, good conductivity and electrochemical stability. It is applied to electrocatalytic oxygen evolution and obtains remarkable results. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is an X-ray diffraction pattern of the Ir / IrO2 catalyst prepared in Example 1 of the present invention;
[0031] Figure 2 This is a transmission electron micrograph of the Ir / IrO2 catalyst prepared in Example 1 of the present invention;
[0032] Figure 3 This is a specific surface area diagram of the Ir / IrO2 catalyst prepared in Example 1 of the present invention;
[0033] Figure 4This is a stability test diagram of the Ir / IrO2 catalyst prepared in Example 1 of the present invention for electrocatalytic oxygen evolution;
[0034] Figure 5 X-ray diffraction patterns of the catalysts prepared in Example 1, Example 17 and Example 18 of the present invention;
[0035] Figure 6 X-ray diffraction patterns of Ir / IrO2 catalysts prepared in Example 1, Comparative Example 4 and Comparative Example 5 of the present invention;
[0036] Figure 7 This is a comparison diagram of the LSV of the catalysts prepared in Example 1, Example 2 and Example 3 of the present invention for electrocatalytic oxygen evolution;
[0037] Figure 8 This is a comparison chart of the LSV of the catalysts prepared in Example 1, Example 4, Example 5 and Example 6 of the present invention for electrocatalytic oxygen evolution;
[0038] Fig. 9 This is a comparison chart of the LSV of the catalysts prepared in Example 1, Example 7, Example 8 and Example 9 of the present invention for electrocatalytic oxygen evolution;
[0039] Fig.10 This is a comparison chart of LSV of the catalysts prepared in Example 1, Example 10, Example 11, Example 12 and Example 13 of the present invention for electrocatalytic oxygen evolution;
[0040] Fig.11 This is a LSV comparison diagram of the catalysts prepared in Example 1, Example 14, Example 15 and Example 16 of the present invention for electrocatalytic oxygen evolution;
[0041] Fig.12 This is a comparison chart of LSV of the catalysts prepared in Example 1, Example 17 and Example 18 of the present invention for electrocatalytic oxygen evolution;
[0042] Fig.13 This is a LSV comparison diagram of the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention for electrocatalytic oxygen evolution;
[0043] Fig.14 This is a comparison diagram of LSV for electrocatalytic oxygen evolution of Example 1 and Comparative Example 3 described in the present invention;
[0044] Fig.15 1 is a comparison chart of LSV for electrocatalytic oxygen evolution of Ir / IrO2 catalysts prepared in Example 1, Comparative Example 4 and Comparative Example 5 of the present invention. DETAILED DESCRIPTION
[0045] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0046] like Figure 1 , Figure 2 As shown, the present invention provides an iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution, specifically comprising: an XRD spectrum of the iridium-oxygen composite nanocatalyst includes a (101) crystal plane diffraction peak of IrO2, but no (110) crystal plane diffraction peak; also includes a (311) crystal plane diffraction peak and a (222) crystal plane diffraction peak of Ir, but no (211) crystal plane diffraction peak; the particle size of the iridium-oxygen composite nanocatalyst is 2 to 5 nm, and the surface of the iridium-oxygen composite nanocatalyst exposes a (111) crystal plane.
[0047] The present invention also provides a method for preparing an iridium-oxygen complex nanocatalyst for electrocatalytic oxygen evolution, comprising: adding an organic ligand to chloroiridic acid and continuously stirring, adjusting the pH to react, vacuum freeze-drying to obtain a precursor after the reaction is completed, calcining the precursor, and washing to obtain the iridium-oxygen complex nanocatalyst, wherein the final product is a black iridium-oxygen complex black powder with a particle size of 2-5 nm; the method specifically comprises the following steps:
[0048] Step 1, dissolving a certain amount of chloroiridic acid in ultrapure water, adding a certain amount of organic acid, stirring the reaction at a certain temperature for a certain time, adding sodium hydroxide solution to adjust the pH and continuing stirring;
[0049] Step 2: After stirring is completed, pour the reaction solution into a petri dish and place it in a vacuum freeze dryer overnight to completely lose water to obtain a precursor, place it in a crucible and calcine it in a muffle furnace at a set temperature and time. After calcination, grind it thoroughly, wash it with ethanol and ultrapure water several times, and dry it to obtain an iridium oxygen complex catalyst.
[0050] In the present invention, by controlling the amount of different chloroiridic acids added, different organic acids, adjusting the pH of the reaction solution, the reaction time, the reaction temperature and other parameters, it is beneficial to obtain ultra-small nanoparticles with a particle size of 2-5 nanometers.
[0051] In another embodiment, the specific preparation method in step 1 includes: first, dissolving 0.1-0.3 g of chloroiridic acid solution in 30 mL of ultrapure water, adding 0.2-0.8 g of an organic acid under stirring, heating and stirring at 90° C. for 30 min; adding 2 M sodium hydroxide solution to the solution to adjust the pH to 2-11, and continuing stirring for 3 h;
[0052] The specific preparation method in step 2 includes: after the reaction is completed, placing the reaction liquid in a vacuum freeze drying box and drying it in a vacuum environment for 24 hours, and taking out the precursor powder after the water is completely lost, and grinding it; after sufficient grinding, calcining it at a temperature of 300-700°C for 10-60 minutes, washing it with ethanol and water after the calcination is completed, and drying it to obtain an iridium oxygen complex catalyst.
[0053] In another embodiment, in step 1, the chloroiridic acid solution is a solution in which the iridium content is 35% dissolved in HCl, the concentration of the sodium hydroxide solution used is 2 mol / L, and the organic acid is L-aspartic acid, oxalic acid or succinic acid.
[0054] In another embodiment, the specific preparation method in step 1 includes: the preparation method of the reaction solution is: weigh 0.2g of chloroiridic acid and 0.4g of L-aspartic acid, dissolve in 30mL of ultrapure water and stir at 90°C for 30min; adjust the pH of the reaction solution to 9 with 2M sodium hydroxide solution and continue stirring for 3h;
[0055] In another embodiment, in step 2, vacuum drying is pre-freezing at -30°C and vacuum drying at 20°C.
[0056] In another embodiment, in step 2, the reaction solution prepared in step 1 is poured into a glass culture dish and pre-frozen at -30°C for 5 hours until it becomes solid, and then vacuum dried at 20°C for 12 hours to remove moisture to obtain a precursor.
[0057] In another embodiment, in step 2, the calcination temperature is 300°C-700°C.
[0058] In another embodiment, in step 2, the calcination time is 10 to 60 minutes.
[0059] In another embodiment, in step 2, the vacuum-dried precursor is placed in a crucible and calcined in a muffle furnace at 600° C. for 30 minutes to obtain a crude product.
[0060] In another embodiment, in step 2, washing refers to washing with anhydrous ethanol and ultrapure water for 3 times respectively and centrifuging.
[0061] In another embodiment, in step 2, drying refers to drying at 90° C. for 4 hours in an electric heated forced air drying oven.
[0062] The present invention also provides an application of an iridium-oxygen composite nanocatalyst in electrocatalytic oxygen evolution at an anode. The specific method is: using the iridium-oxygen composite nanocatalyst prepared as an anode catalyst for electrocatalytic oxygen evolution, and comparing the electrocatalytic oxygen evolution at a current density of 10 mA cm -2 The overpotential at that time is used to measure the quality of the catalyst.
[0063] The present invention will be further described below in conjunction with specific embodiments.
[0064] Example 1
[0065] A method for synthesizing an ultrafine-sized iridium-oxygen composite nanocatalyst comprises the following steps:
[0066] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an ultrafine iridium-oxygen composite nanocatalyst.
[0067] Example 2
[0068] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0069] First, 0.1g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The reaction solution was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide nanocatalyst.
[0070] Example 3
[0071] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0072] First, 0.3g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The reaction solution was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the precursor was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide nanocatalyst.
[0073] Example 4
[0074] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0075] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.2g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0076] Example 5
[0077] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0078] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.6g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0079] Example 6
[0080] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0081] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.8g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0082] Example 7
[0083] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0084] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 2.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0085] Example 8
[0086] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0087] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 5.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0088] Example 9
[0089] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0090] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 11.0. The reaction solution was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0091] Example 10
[0092] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0093] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 300℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0094] Embodiment 11
[0095] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0096] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 400℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0097] Example 12
[0098] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0099] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 500℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0100] Embodiment 13
[0101] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0102] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 700℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0103] Embodiment 14
[0104] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0105] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The reaction solution was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The reaction solution was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 10min. After calcination, the precursor was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide complex nanocatalyst.
[0106] Embodiment 15
[0107] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0108] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 20min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide complex nanocatalyst.
[0109] Example 16
[0110] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0111] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 60min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide complex nanocatalyst.
[0112] Embodiment 17
[0113] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0114] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of oxalic acid was added. The mixture was stirred magnetically at 90℃ for 30min. A 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0, and the mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxide complex nanocatalyst.
[0115] Embodiment 18
[0116] A preparation method of an iridium-oxygen composite nanocatalyst comprises the following steps:
[0117] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, 0.4g of succinic acid was added, and magnetic stirring was performed at 90°C for 30min. A 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0, and magnetic stirring was continued at 90°C for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30°C for 5h until the reaction solution became solid, and vacuum dried at 20°C for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600°C in a muffle furnace for 30min. After calcination, it was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90°C for 4h to obtain an iridium oxide complex nanocatalyst.
[0118] Comparative Example 1
[0119] The catalyst is prepared by changing the added ligand and reducing agent, comprising the following steps:
[0120] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of citric acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium-oxygen composite nanocatalyst.
[0121] Comparative Example 2
[0122] The catalyst is prepared by changing the added ligand and reducing agent, comprising the following steps:
[0123] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, 0.4g of formic acid was added, and magnetic stirring was performed at 90℃ for 30min. A 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0, and magnetic stirring was continued at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid, and vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 600℃ in a muffle furnace for 30min. After calcination, it was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an iridium oxygen composite nanocatalyst.
[0124] Comparative Example 3
[0125] The commercial iridium black catalyst and the commercial IrO2 catalyst used were purchased from Anhui Masushui New Energy Technology Co., Ltd., with product numbers: SS-Ir-2002; SS-IrO2-3001, respectively.
[0126] Comparative Example 4
[0127] The catalyst is prepared by changing the calcination temperature, comprising the following steps:
[0128] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 200℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an ultrafine iridium-oxygen composite nanocatalyst.
[0129] Comparative Example 5
[0130] The catalyst is prepared by changing the calcination temperature, comprising the following steps:
[0131] First, 0.2g of chloroiridic acid was dissolved in 20mL of ultrapure water, and 0.4g of L-aspartic acid was added. The mixture was stirred magnetically at 90℃ for 30min, and 2M sodium hydroxide solution was added to adjust the pH of the reaction solution to 8.0. The mixture was stirred magnetically at 90℃ for 3h. After stirring, the reaction solution was poured into a petri dish and placed in a vacuum freeze dryer at -30℃ for 5h until the reaction solution became solid. The mixture was vacuum dried at 20℃ for 12h until the water was completely volatilized. The dried precursor was taken out and placed in a crucible and calcined at 800℃ in a muffle furnace for 30min. After calcination, the mixture was fully ground and washed three times with ethanol and ultrapure water respectively, and then placed in an electric blast drying oven at 90℃ for 4h to obtain an ultrafine iridium-oxygen composite nanocatalyst.
[0132] Test Case
[0133] XRD test instrument: Japan-Rigaku-SmartLab 9kW, Cu-Kα diffraction TEM+Mapping test instrument: Use JEOL JEM-ARM200F Cs-corrected S / TEM for HAADF-STEM tomography; BET test instrument and test method: Use Micromeritics ASAP 2020 (BELSORP max) to collect N2 gas absorption / desorption data, and obtain the specific surface area and pore distribution by implementing the Brunauer-Emmett-Teller (BET) and Barrett Joyner-Halenda (BJH) methods respectively.
[0134] Ultrafine iridium oxygen composite nanoparticle catalyst is used for anode electrocatalytic oxygen evolution. The specific application method is: weigh 10 mg of the catalyst prepared in Examples 1 to 18 and the catalyst prepared in Comparative Examples 1, 2, 4 and 5, respectively, add 109 μL 5% Nafion solution, 542 μL ultrapure water, 1349 μL isopropanol to make ink and ultrasonicate for 2 hours to mix evenly. Use a pipette to take 15 μ Link solution and drip it on the surface of the glassy carbon electrode three times and dry it with an infrared drying lamp as the anode, a saturated calomel electrode as the reference electrode, a platinum sheet as the auxiliary electrode, and a 0.5 M H2SO4 solution as the electrolyte. Test its OER performance at room temperature.
[0135] The catalyst prepared in Example 1 was compared with a commercial iridium-based catalyst (Comparative Example 3). The specific application method was as follows: 10 mg of the catalyst prepared in Example 1, iridium black catalyst and commercial IrO2 catalyst were weighed respectively, and 109 μL of 5% Nafion solution, 542 μL of ultrapure water and 1349 μL of isopropanol were added to form ink and ultrasonicated for 2 hours to mix evenly. 15 μL Link solution was applied to the surface of the glassy carbon electrode three times with a pipette gun and dried with an infrared drying lamp as an anode, a saturated calomel electrode as a reference electrode, a platinum sheet as an auxiliary electrode, and an electrolyte of 0.5 M H2SO4 solution. Its OER performance was tested at room temperature.
[0136] The nanoparticle catalyst prepared in Example 1 was characterized, and the XRD pattern was as follows: Figure 1 As shown, in order to confirm the formation of the iridium-oxygen complex structure, a typical X-ray diffraction (XRD) test of Ir / IrO2 was carried out. There were six obvious peaks at 34.6°, 40.6°, 47.0°, 69.2°, 84.1° and 88.1°, corresponding to (101), (111), (200), (220), (311) and (222) crystal planes, respectively. The results calculated based on the half-peak width showed that the average particle size of the catalyst was 2.32 nm, indicating that extremely small-sized nanoparticles were synthesized; as shown in FIG. Figure 2 As shown in the figure, the crystal plane spacing is measured to be 0.22 nm through transmission electron microscopy (TEM) images, which shows that the catalyst exposes the (111) crystal plane. Many papers have previously reported that this crystal plane has a significant promoting effect on reducing the overpotential of OER; Figure 3 As shown in the figure, the specific surface area (BET) results show that the specific surface area of the catalyst is 35.665 m 2 g -1 , the average pore size is 5.4nm; Figure 4 As shown, the catalyst prepared in Example 1 was tested for stability, and the overpotential increased by only 23 mV after CV cycle 30000 cycles; Figure 5As shown, the compounds synthesized by the three ligands have the same characteristic peaks, such as Figure 6 As shown, the XRD results show that when the calcination temperature is 200°C, no iridium dioxide peak appears, indicating that the product at this calcination temperature contains only iridium. When the calcination temperature is 800°C, the iridium peak in the product disappears, leaving only the characteristic peak of iridium dioxide, indicating that the product at this calcination temperature contains only iridium dioxide.
[0137] As shown in Table 1, the results of the mapping test show that the prepared catalyst has a high purity and contains only two elements, iridium and oxygen.
[0138] Table 1 Mapping test results
[0139]
[0140]
[0141] like Figure 7 As shown in Figure 2, when other synthesis conditions remain unchanged, the prepared catalyst can be used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 259mV and 270mV respectively; Figure 8 As shown in Figure 2, when other synthesis conditions remain unchanged, the prepared catalyst can be used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 238mV, 254mV and 265mV respectively; Fig. 9 As shown in Figure 2, under the condition that other synthesis conditions remain unchanged, the solution pH is adjusted to 8, 11, 2 and 5 by adding different amounts of sodium carbonate solution. The prepared catalyst is used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 237mV, 250mV and 259mV respectively; Fig.10 As shown in Figure 2, when other synthesis conditions remain unchanged, the calcination temperature is changed to 300℃, 400℃, 700℃, 600℃ and 500℃ respectively. The prepared catalysts can be used for OER at a current density of 10mA cm -2 When , the overpotentials are 295mV, 283mV, 242mV, 235mV and 263mV respectively; Fig.11 As shown in the figure, when other synthesis conditions remain unchanged, the calcination time is changed to 10 min, 20 min, 60 min and 30 min respectively. The prepared catalysts are used for OER at a current density of 10 mA cm -2 When , the overpotentials are 278mV, 235mV, 269mV and 262mV respectively; Fig.12 As shown in Figure 2, when other synthesis conditions remain unchanged, the prepared catalyst can be used for OER at a current density of 10 mA cm-2 When , the overpotentials are 235mV, 276mV and 292mV respectively; Fig.13 As shown in Figure 2, when other synthesis conditions remain unchanged, the prepared catalyst can be used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 281mV and 303mV respectively; Fig.14 As shown in Figure 2, when other synthesis conditions remain unchanged, the prepared catalyst can be used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 262mV and 290mV respectively. Fig.15 As shown in Figure 2, when other synthesis conditions remain unchanged, the calcination temperature is changed to 600℃, 800℃ and 200℃ respectively. The prepared catalysts can be used for OER at a current density of 10 mA cm -2 When , the overpotentials are 235mV, 288mV and 309mV respectively.
[0142] The above charts show that the iridium-oxygen composite nanoparticle catalyst provided by the present invention has the characteristics of small and uniform particles. The catalysts prepared in all embodiments have achieved significant results in OER, with a current density of 10 mA cm -2 The overpotentials were all less than 300 mV; in particular, the catalyst prepared in Example 1 had an overpotential of only 235 mV, which was far superior to commercial iridium-based catalysts and had excellent stability. After 30,000 continuous CV cycles, the overpotential increased by only 23 mV.
Claims
1. An iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution, characterized in that: include: The XRD spectrum of the iridium-oxygen composite nanocatalyst includes a (101) crystal plane diffraction peak of IrO2 and no (110) crystal plane diffraction peak; and Includes the (311) crystal plane diffraction peak and (222) crystal plane diffraction peak of Ir, but no (211) crystal plane diffraction peak; The method for preparing the iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution comprises the following steps: Step 1, adding an organic ligand to chloroiridic acid, stirring continuously, and adjusting the pH to react; Step 2: After the reaction is completed, vacuum freeze-drying is performed to obtain a precursor; Step 3, calcining the precursor and washing it to obtain the iridium-oxygen composite nanocatalyst; The organic ligand is L-aspartic acid; In the step three, the calcination conditions include: the calcination temperature range is 300° C. to 700° C., and the calcination time range is 10 to 60 minutes.
2. The iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution according to claim 1, characterized in that: The particle size of the iridium-oxygen composite nanocatalyst is 2-5 nm.
3. The iridium-oxygen composite nanocatalyst for electrocatalytic oxygen evolution according to claim 1 or 2, characterized in that: The iridium-oxygen composite nanocatalyst has exposed (111) crystal planes on its surface.
4. Use of the iridium-oxygen composite nanocatalyst as described in any one of claims 1 to 3 in anode electrocatalytic oxygen evolution.