A road brick and its preparation method
By using solid waste materials such as sand washing tailings, alkali residue, fly ash and stones, combined with semi-sintered brick technology and high-temperature sintering technology, the problems of time, labor and environmental pollution in the production process of traditional street bricks have been solved, and the problem of environmental pollution has been achieved. Efficient resource utilization and performance improvement.
Patent Information
- Application Number
- CN202410433406.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-04-11
AI Technical Summary
The production process of traditional street bricks is time-consuming, labor-intensive, high-cost, generates a large amount of wastewater and solid waste, has an impact on the environment, and causes serious waste of raw materials and energy.
Using solid waste materials such as sand washing tailings, alkali residue, fly ash, gravel and cement, pavement bricks are prepared through the semi-sintered brick process. The alkali-stimulated reaction of the alkali residue and fly ash is used to form cementing substances to improve strength and durability. , and improve the compressive strength and anti-skid properties through high-temperature sintering and pressing.
Effective resource utilization of solid waste reduces environmental pollution, reduces transportation costs, and improves the compressive strength and anti-skid performance of sidewalk bricks, which has good ecological and economic effects.
Smart Images

Figure GDA0005019230490000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road bricks, in particular to a road brick and a preparation method thereof. Background Art
[0002] Shilianghe Reservoir is the largest artificial reservoir in Jiangsu Province. Due to the disorderly sand mining and excessive development in the past, the ecological environment of the reservoir has been severely damaged. Sand washing tailings are waste generated in the sand washing process. If these tailings are not properly handled, they will have a negative impact on the water quality and ecological environment of the reservoir.
[0003] Alkali residue is the alkaline waste residue discharged from the process of alkali production and alkali treatment in industrial production. It mainly includes waste residues with calcium salts such as calcium carbonate, calcium sulfate, and calcium chloride as the main components, and also contains a small amount of sulfur dioxide, magnesium salt, sodium salt and SiO 2 It is estimated that for every ton of Na2CO3 produced by the ammonia-soda process, 0.3 tons of alkali slag will be produced. The accumulation of alkali slag occupies land resources and pollutes the environment. The alkali slag is highly alkaline with a pH value of about 10-12. The particle size of the alkali slag is very fine. After firing, CaO is produced, which has cementitious properties.
[0004] Fly ash is mainly derived from the main solid waste discharged from coal-fired power plants. It is the fine ash produced in the flue gas after coal combustion. The main components of fly ash are silicon oxide, aluminum oxide and iron oxide, and it also contains a small amount of carbon, calcium, magnesium and other elements. As an important industrial waste residue, fly ash is fully utilized in different fields.
[0005] Sidewalk bricks play a very important role in urban construction, but there are still some problems. Traditional sidewalk bricks are not only time-consuming and labor-intensive to produce, but also relatively costly. A large amount of wastewater, waste and solid waste will be generated in the production process, which has a certain impact on the environment. There is also waste of raw materials and energy.
[0006] Chinese invention patent CN202211464640.9 discloses a sidewalk brick and a preparation method thereof. Lake sediment, gravel, sand, steel slag, cement, slag powder and alkali activator are mixed to prepare sidewalk bricks to improve the problem of low compressive strength. However, the finished product is high, the materials used are large, the preparation process is relatively complicated, the produced sidewalk bricks are heavy, and the transportation of finished products increases. Therefore, a sidewalk brick and a preparation method thereof are provided. Summary of the invention
[0007] The purpose of the present invention is to provide a pavement brick and a preparation method thereof in view of the defects of the prior art, so as to solve the problems raised by the above-mentioned background technology.
[0008] To achieve the above object, the present invention provides the following technical solution: a road brick, comprising the following raw materials in mass percentage: 10-25% of sand washing tailings, 15-30% of alkali residue, 10-15% of cement, 25-40% of gravel, and 10-20% of fly ash;
[0009] As a preferred technical solution of the present invention, the sand washing tailings account for 20%, the alkali slag accounts for 25%, the cement accounts for 12%, the gravel accounts for 28%, and the fly ash accounts for 15%.
[0010] As a preferred technical solution of the present invention, the sand washing tailings account for 18%, the alkali slag accounts for 27%, the cement accounts for 12%, the gravel accounts for 28%, and the fly ash accounts for 15%.
[0011] As a preferred technical solution of the present invention, the stone particle size is 1 to 4 mm.
[0012] A method for preparing a road brick, the specific steps are as follows:
[0013] S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 70-90r / min and the stirring time is 2-5 minutes to obtain a mixed raw material;
[0014] S2: putting the mixed raw materials into a mold to prepare semi-fired bricks;
[0015] S3: putting the prepared semi-sintered brick into a pressing machine for preliminary pressing;
[0016] S4: Preliminary sintering of the pressed semi-fired bricks at a temperature of 800-1000°C;
[0017] S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements;
[0018] S6: The cooled semi-sintered bricks are subjected to secondary pressing and then placed in a temperature of 1000-1200°C for secondary sintering;
[0019] S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.
[0020] As a preferred technical solution of the present invention, the preliminary pressing in step S3 is performed by hydraulic forming using a hydraulic press, and the required strength is 15 to 20 MPa.
[0021] As a preferred technical solution of the present invention, the secondary pressing in step S6 adopts hydraulic forming by a hydraulic press, and the required strength is 20-25 MPa.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention uses fly ash, alkali slag, gravel, and sand washing tailings as main raw materials with a large dosage. The fly ash and alkali slag can replace a part of cement to play a bonding role. The alkali slag can react with silicates and aluminates in the fly ash to form a bonding material, which helps to improve the strength and durability of the road bricks.
[0024] 2. During the high-temperature sintering process, the silicates, aluminates, etc. in the raw materials will partially melt, causing chemical reactions inside the material, such as solid-phase reactions, to form silicate minerals, further improving the performance and durability of the road bricks.
[0025] 3. The present invention adopts the semi-fired brick process. The surface of the semi-fired brick has a certain degree of roughness, which increases the anti-skid property of the road brick and reduces the risk of sliding when pedestrians and vehicles are walking. The semi-fired brick is lighter, which reduces the transportation cost.
[0026] 4. The formula of the present invention uses solid waste as the main raw material, which can effectively utilize solid waste resources and reduce environmental pollution. At the same time, it can also provide higher compressive strength and anti-slip performance, and has a good ecological and economic effect. DETAILED DESCRIPTION
[0027] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0028] The present invention provides a method for preparing road bricks, comprising the following raw materials in percentage by mass: 10-25% of sand washing tailings, 15-30% of alkali residue, 10-15% of cement, 25-40% of gravel, and 10-20% of fly ash;
[0029] The specific steps are as follows:
[0030] S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 70-90r / min and the stirring time is 2-5 minutes to obtain a mixed raw material;
[0031] S2: putting the mixed raw materials into a mold to prepare semi-fired bricks;
[0032] S3: putting the prepared semi-sintered brick into a pressing machine for preliminary pressing;
[0033] S4: Preliminary sintering of the pressed semi-fired bricks at a temperature of 800-1000°C;
[0034] S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements;
[0035] S6: The cooled semi-sintered bricks are subjected to secondary pressing and then placed in a temperature of 1000-1200°C for secondary sintering;
[0036] S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.
[0037] In the present invention, alkali slag, sand washing tailings and gravel are fully ground and evenly mixed with fly ash. Alkali slag has a high alkaline component and can react with silicate and aluminate in fly ash to form a cementing material, which helps to improve the strength and durability of road bricks. Sand washing tailings have a high sand content and can replace sand. The road bricks prepared therefrom have high strength, good durability and good skid resistance.
[0038] The following is an example of a method for preparing road bricks from semi-fired bricks of the present invention:
[0039] Embodiment 1:
[0040] Sand washing tailings, alkali slag, fly ash, cement and gravel are prepared into road bricks through semi-sintered brick process.
[0041] Their mass fractions are: 20% sand washing tailings, 25% alkali residue, 12% cement, 28% gravel and 15% fly ash;
[0042] Embodiment 1 provides a method for preparing road bricks, comprising the following steps:
[0043] S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 70r / min and the mixing time is 5 minutes;
[0044] S2: putting the mixed raw materials into a mold to prepare semi-fired bricks;
[0045] S3: putting the prepared semi-sintered brick into a pressing machine and performing preliminary pressing at 15 MPa;
[0046] S4: preliminarily sintering the pressed semi-fired bricks at a temperature of 800°C;
[0047] S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements;
[0048] S6: The cooled semi-fired bricks are subjected to secondary pressing at 20 MPa and then subjected to secondary sintering at 1000°C;
[0049] S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.
[0050] The compressive strength of the road bricks obtained by this method is 24MPa at 14d, and the strength at 28d is 28MPa.
[0051] Embodiment 2:
[0052] The difference between the raw materials and Example 1 is:
[0053] Their mass fractions are: 18% sand washing tailings, 27% alkali residue, 12% cement, 28% gravel and 15% fly ash;
[0054] Embodiment 2 provides a method for preparing a road brick, comprising the following steps:
[0055] S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 80r / min and the mixing time is 4 minutes;
[0056] S2: putting the mixed raw materials into a mold to prepare semi-fired bricks;
[0057] S3: putting the prepared semi-sintered brick into a pressing machine and performing preliminary pressing at 18 MPa;
[0058] S4: preliminarily sintering the pressed semi-fired bricks at a temperature of 900°C;
[0059] S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements;
[0060] S6: The cooled semi-sintered bricks are subjected to secondary pressing at 23 MPa and then subjected to secondary sintering at 1100°C;
[0061] S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.
[0062] The compressive strength of the road bricks obtained by this method is 24.69MPa at 14d, and the strength at 28d is 29.98MPa.
[0063] Embodiment 3:
[0064] The difference between the raw materials and Example 1 is:
[0065] Their mass fractions are: 25% sand washing tailings, 19% alkali slag, 11% cement, 28% gravel and 17%
[0066] Fly ash;
[0067] Embodiment 3 provides a method for preparing a road brick, comprising the following steps:
[0068] S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 90r / min and the mixing time is 3 minutes;
[0069] S2: putting the mixed raw materials into a mold to prepare semi-fired bricks;
[0070] S3: putting the prepared semi-sintered brick into a pressing machine and performing preliminary pressing at 20 MPa;
[0071] S4: preliminarily sintering the pressed semi-fired bricks at a temperature of 1000°C;
[0072] S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements;
[0073] S6: The cooled semi-fired bricks are subjected to secondary pressing at 25 MPa and then subjected to secondary sintering at 1200°C;
[0074] S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.
[0075] The compressive strength of the road bricks obtained by this method is 23.3MPa at 14d, and the strength at 28d is 27.5MPa.
[0076] The example results are shown in the following table:
[0077]
[0078] The present invention uses fly ash, alkali slag, gravel and sand washing tailings as main raw materials with a large dosage. The fly ash and alkali slag can replace a part of cement to play a bonding role. The alkali slag can react with silicate and aluminate in the fly ash to form a bonding material, which helps to improve the strength and durability of the road bricks.
[0079] During the high-temperature sintering process, silicates, aluminates, etc. in the raw materials will partially melt, causing chemical reactions inside the material, such as solid-phase reactions, to form silicate minerals, further improving the performance and durability of the road bricks. The present invention adopts a semi-fired brick process, and the surface of the semi-fired brick has a certain degree of roughness, which increases the anti-skid property of the road bricks and reduces the risk of slipping when pedestrians and vehicles are walking. Semi-fired bricks are lighter, reducing transportation costs. The formula of the present invention uses solid waste as the main raw material, which can effectively utilize solid waste resources and reduce environmental pollution. At the same time, it can also provide higher compressive strength and anti-skid performance, and has a good ecological and economic effect.
[0080] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention.
Claims
1. A method for preparing road bricks, Features: The raw materials are composed of the following mass percentages: 10-25% of sand washing tailings, 15-30% of alkali residue, 10-15% of cement, 25-40% of gravel, and 10-20% of fly ash; the gravel particle size is 1-4 mm; The specific preparation method of road bricks is as follows: S1: Put fly ash, alkali slag, gravel, sand washing tailings and cement into a mixer according to the proportion and mix them. The mixer speed is 70-90r / min and the stirring time is 2-5 minutes to obtain a mixed raw material; S2: putting the mixed raw materials into a mold to prepare semi-fired bricks; S3: Put the prepared semi-sintered bricks into a press for preliminary pressing; the preliminary pressing adopts hydraulic forming by a hydraulic press, and the required strength is 15-20MPa; S4: Preliminary sintering of the pressed semi-fired bricks at a temperature of 800-1000°C; S5: Cool the semi-fired bricks that have been initially sintered and check the quality to ensure that they meet the standard requirements; S6: The cooled semi-sintered bricks are pressed for the second time and then placed in a temperature of 1000-1200°C for secondary sintering; the secondary pressing is hydraulically formed by a hydraulic press, and the required strength is 20-25MPa S7: After sintering is completed, maintain a certain pressure and time to determine the density of the bricks.