A composite material based on modified heavy calcium carbonate and its application

Through the preparation of modified heavy calcium carbonate, combined with halogen-free flame retardant elements and specific groups, the environmental and health risks when composite materials are burned are solved, efficient flame retardant performance and physical properties are improved, and production costs are reduced.

CN118206842BActive Publication Date: 2024-10-18HUNAN BAIYU TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410326926.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2024-10-18
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

Existing composite materials emit large amounts of smoke, produce toxic and harmful gases and carcinogens when burned, affecting the environment and human health, and the use of flame retardants poses environmental and health risks.

Method used

Using modified heavy calcium carbonate, intermediates containing halogen-free flame retardant elements nitrogen, phosphorus and silicon are prepared under nitrogen protection, and combined with long alkyl chains, benzene rings, amide groups and ester groups to form highly dispersible composite materials. Enhance its flame retardant performance and physical properties.

Benefits of technology

It achieves excellent flame retardant properties of composite materials, improves dimensional stability, hardness and gloss, reduces production costs, reduces the generation of harmful gases, and improves material safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004752337930000031
    Figure BDA0004752337930000031
  • Figure BDA0004752337930000032
    Figure BDA0004752337930000032
  • Figure BDA0004752337930000041
    Figure BDA0004752337930000041
Patent Text Reader

Abstract

The invention discloses a composite material and application based on modified heavy calcium carbonate, belonging to the technical field of composite materials. The raw materials of the composite material include: 45-55 parts of high-impact polystyrene, 25-35 parts of toughening agent, 9-12 parts of modified heavy calcium carbonate, 3-5 parts of plasticizer, 0.1-0.5 parts of antioxidant, 0.5-1.5 parts of antistatic agent, 0.1-0.3 parts of lubricant, 1-2 parts of toner, 0.01-0.03 parts of diisopropylbenzene peroxide. Long alkyl chain, benzene ring and amide group etc. improve the compatibility of modified heavy calcium carbonate in the system, and the chemical reaction between modified heavy calcium carbonate and polymer further increases the dispersibility of modified heavy calcium carbonate in the system, therefore, highly dispersed modified heavy calcium carbonate makes the composite material of the present invention have excellent flame retardant performance, improves the dimensional stability, hardness, glossiness and flatness of the composite material, and further reduces the production cost of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials, and in particular, relates to a composite material based on modified heavy calcium carbonate and its application. Background Art

[0002] Heavy calcium carbonate, referred to as heavy calcium, is a white powder made of calcium carbonate as the main component and calcite as the raw material. It plays an important role in many industrial fields. As an important filler in the rubber industry, heavy calcium can increase the volume of rubber products, reduce the use of expensive natural rubber, and thus reduce costs; in addition, it can also improve the tensile strength, tear strength and wear resistance of rubber products. In the plastics industry, heavy calcium can improve the dimensional stability and hardness of plastic products, as well as the gloss and flatness of the products. For specific requirements, such as whiteness and stability after high-temperature heating, high-quality heavy calcium powder can also meet these needs. In addition to rubber and plastics, heavy calcium is also widely used in many daily chemical industries such as coatings, cables, building supplies, and textiles. In these fields, the main role of heavy calcium is still as a filler, increasing the volume of products, reducing costs, and helping to improve certain physical and chemical properties of products.

[0003] Composite materials such as rubber, plastic and coating are widely used in daily production, and most of the composite materials are flammable substances. Although good flame retardant effects can be obtained by adding low-cost and high-efficiency halogen-containing flame retardants in the existing technology, they have problems such as large smoke production, generation of toxic and harmful gases and carcinogens during combustion, and significant impact on the environment and human body. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a composite material based on modified heavy calcium carbonate and its application.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A composite material based on modified heavy calcium carbonate comprises the following raw materials in parts by weight: 45-55 parts of high impact polystyrene, 25-35 parts of toughening agent, 9-12 parts of modified heavy calcium carbonate, 3-5 parts of plasticizer, 0.1-0.5 parts of antioxidant, 0.5-1.5 parts of antistatic agent, 0.1-0.3 parts of lubricant, 1-2 parts of color powder, and 0.01-0.03 parts of dicumyl peroxide;

[0007] Furthermore, the toughening agent is one or more of styrene-butadiene-styrene block copolymer, ethylene-vinyl acetate copolymer, and methyl acrylate-butadiene-styrene copolymer.

[0008] Furthermore, the modified heavy calcium carbonate is prepared by the following steps:

[0009] S1. Under nitrogen protection, guanidine melamine, triethylamine and DMSO (dimethyl sulfoxide) were added to a dry four-necked flask, and the mixture was stirred and mixed evenly. (2-chloroethyl) phosphonic acid diethyl ester was slowly added under stirring, and the mixture was reacted at 80° C. for 3 h. After the reaction, deionized water was added to the reaction solution, and the mixture was stirred and allowed to stand. The organic phase was taken, and the organic phase was washed three times with saturated brine, and then dried over anhydrous magnesium sulfate. After drying, the organic phase was filtered and distilled under reduced pressure to obtain intermediate 1. The amount ratio of guanidine melamine, (2-chloroethyl) phosphonic acid diethyl ester, triethylamine and DMSO was 10.1 g:12 g:8.3 mL:120 mL.

[0010] Under alkaline conditions, -NH2 of guanidine melamine and -Cl of diethyl (2-chloroethyl)phosphonate undergo nucleophilic substitution reaction, and the reaction process is as follows:

[0011]

[0012] S2. Under nitrogen protection, add intermediate 1, 10-undecenoic acid, DMF (N,N-dimethylformamide) and concentrated sulfuric acid in a dry four-necked flask in sequence, stir thoroughly until mixed, heat the oil bath to 120°C, react at this temperature for 8 hours and then cool to room temperature, pour the reactant into 100 mL, 0.1 mol / L sodium bicarbonate aqueous solution, shake and let stand to separate, wash the organic layer with 0.1 mol / L sodium bicarbonate aqueous solution and water in sequence until neutral, add anhydrous magnesium sulfate to dry, and distill under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, 10-undecenoic acid, DMF and concentrated sulfuric acid is 16.6 g:33.3 mL:110 mL:3 mL.

[0013] Under heating conditions and the catalysis of concentrated sulfuric acid, the molar ratio of 10-undecenoic acid to intermediate 1 is controlled to be 3.1-3.4:1, and the amino group of intermediate 1 and the carboxyl group of 10-undecenoic acid undergo a three-molecule dehydration condensation reaction, and the reaction equation is as follows:

[0014]

[0015] S3. Add intermediate 2 and DMF into a fully dried four-necked flask, stir until mixed evenly, heat to 80°C, slowly add 3-glycidyloxypropyltrimethoxysilane (KH560) while stirring, reflux at 80°C for 6 hours after the addition is complete, cool to room temperature after the reaction is completed, and distill under reduced pressure. The whole process is carried out under nitrogen protection to obtain intermediate 3; the usage ratio of intermediate 2, KH560 and DMF is 16.6g:5.7mL:120mL.

[0016] Intermediate 2 and KH560 undergo a nucleophilic substitution reaction under heating conditions. The reaction process is as follows:

[0017]

[0018] S4, pour heavy calcium carbonate and deionized water into a beaker, ultrasonically disperse for 30 minutes, pour into a three-necked flask, start stirring and heating, keep the mixture temperature at 65°C; then, mix DMF and intermediate 3 evenly and slowly add them into the three-necked flask, continue heating and stirring at 65°C for 10 hours after the addition is complete, finally cool to room temperature, filter the mixture, wash with anhydrous ethanol 3 times, and after washing, vacuum dry the product at 80°C for 12 hours to obtain modified heavy calcium carbonate. The mass ratio of intermediate 3 to heavy calcium carbonate is 3:1.

[0019] Modified heavy calcium carbonate contains halogen-free flame retardant elements nitrogen, phosphorus and silicon, which work synergistically to give the composite material excellent flame retardant properties; modified heavy calcium carbonate improves the dimensional stability and hardness of the composite material, while also improving the gloss and smoothness of the composite material. In addition, it also reduces the production cost of the composite material.

[0020] The trimethoxysilane on the modified heavy calcium carbonate undergoes hydrolysis and condensation to form Si-O-Si and Si-OH, wherein the hydroxyl group in the silanol group can form a hydrogen bond with the hydroxyl group on the surface of the heavy calcium carbonate, and then dehydrate and condense to form a covalent bond, thereby greatly improving the dispersion uniformity of the heavy calcium carbonate; in addition, the multiple long alkyl chains on the structure of the modified heavy calcium carbonate make its surface hydrophobic, reduce the intermolecular force, and reduce the agglomeration between the heavy calcium carbonate particles; the long alkyl chain, benzene ring, amide group and ester group have good compatibility with the polymer, and enhance the effect between the interfaces; the modified heavy calcium carbonate also contains multiple terminal carbon-carbon double bonds, which react chemically with the unreacted carbon-carbon double bonds at the end of the polymer under the action of a trace amount of diisopropylbenzene peroxide, which can not only further improve the dispersibility of the modified heavy calcium carbonate, but also make it stably exist in the composite material, improve the dimensional stability, hardness, glossiness and flatness of the composite material, and give the composite material excellent and stable flame retardant properties.

[0021] Furthermore, the plasticizer is one or more of di(2-ethylhexyl) phthalate, dibutyl phthalate, dioctyl phthalate, and chlorinated paraffin.

[0022] Furthermore, the antioxidant is one or a combination of antioxidant 1010, antioxidant 1076, antioxidant DLTP and antioxidant 168.

[0023] Furthermore, the antistatic agent is an ethoxylated alkylamine antistatic agent.

[0024] Furthermore, the lubricant is one or more of polyethylene wax, ethylene stearamide, ethylene bis stearamide, and paraffin wax.

[0025] The invention also discloses application of a composite material based on modified heavy calcium carbonate in the preparation of household appliances, automobiles and toys.

[0026] The beneficial effects of the present invention are as follows: the presence of long alkyl chains, benzene rings, amide groups and ester groups improves the compatibility of the modified heavy calcium carbonate in the system, and the chemical reaction between the modified heavy calcium carbonate and the polymer further increases the dispersibility of the modified heavy calcium carbonate in the system. Therefore, the highly dispersed modified heavy calcium carbonate containing nitrogen, phosphorus, silicon and halogen-free flame retardant elements enables the composite material of the present invention to have excellent flame retardant properties, while improving the dimensional stability, hardness, glossiness and flatness of the composite material. In addition, the production cost of the composite material is also reduced. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] The specific steps for preparing modified heavy calcium carbonate are as follows:

[0030] S1, under nitrogen protection, 10.1g of guanidine melamine, 8.3mL of triethylamine and 120mL of DMSO were added to a dry 250mL four-necked flask, and the mixture was stirred and mixed evenly. 12g of diethyl (2-chloroethyl)phosphonate was slowly added under stirring, and the mixture was reacted at 80°C for 3h. After the reaction, deionized water was added to the reaction solution, and the mixture was stirred and allowed to stand. The organic phase was taken, and the organic phase was washed 3 times with saturated brine, dried over anhydrous magnesium sulfate, filtered, and finally distilled under reduced pressure to obtain intermediate 1;

[0031] S2, under nitrogen protection, 16.6 g of intermediate 1, 33.3 mL of 10-undecenoic acid, 110 mL of DMF, and 3 mL of concentrated sulfuric acid were added to a dry 250 mL four-necked flask in sequence, and the mixture was stirred thoroughly until uniformly mixed. The oil bath was heated to 120° C., reacted at this temperature for 8 h, and then cooled to room temperature. The reactant was poured into 100 mL of a 0.1 mol / L aqueous sodium bicarbonate solution, and allowed to stand for stratification after shaking. The organic layer was washed with a 0.1 mol / L aqueous sodium bicarbonate solution and water in sequence until neutral, dried with anhydrous magnesium sulfate, and distilled under reduced pressure to obtain intermediate 2;

[0032] S3, 16.6g of intermediate 2 and 120mL of DMF were added to a fully dried 250mL four-necked flask, stirred until uniformly mixed, heated to 80°C, and 5.7mL of KH560 was slowly added while stirring. After the addition was completed, the mixture was refluxed at 80°C for 6h. After the reaction was completed, the mixture was cooled to room temperature and distilled under reduced pressure. The whole process was carried out under nitrogen protection to obtain intermediate 3;

[0033] S4. Pour 1g of heavy calcium carbonate and 20mL of deionized water into a beaker, ultrasonically disperse for 30min, then pour into a 250mL three-necked flask, start stirring and heating to keep the temperature of the mixture at 65°C; then, mix 90mL of DMF and 3g of intermediate 3 evenly and slowly add them into the three-necked flask. After the addition is complete, continue heating and stirring at 65°C for 10h, finally cool to room temperature, filter the mixture, wash with anhydrous ethanol 3 times, and after washing, vacuum dry the product at 80°C for 12h to obtain modified heavy calcium carbonate.

[0034] Example 2

[0035] The composite material based on modified heavy calcium carbonate is prepared in the following specific steps:

[0036] 9 parts of the modified heavy calcium carbonate of Example 1, 0.5 parts of Clariant antistatic agent Hostastat FA 68V, 0.1 parts of antioxidant 1076, 0.1 parts of ethylene stearamide, 1 part of phthalocyanine green and 0.01 parts of dicumyl peroxide are mixed uniformly to obtain a premix; the premix and 45 parts of high-impact polystyrene, 25 parts of ethylene-vinyl acetate copolymer and 3 parts of di(2-ethylhexyl) phthalate are fully mixed by a high-speed mixer, and then formed and granulated by a parallel twin-screw extruder to obtain a composite material based on modified heavy calcium carbonate.

[0037] Example 3

[0038] The composite material based on modified heavy calcium carbonate is prepared in the following specific steps:

[0039] 10 parts of the modified heavy calcium carbonate of Example 1, 0.7 parts of Clariant antistatic agent Hostastat FA 68V, 0.15 parts of antioxidant 1010 and 0.15 parts of antioxidant DLTP compound, 0.2 parts of ethylene bisstearamide, 1.5 parts of phthalocyanine green and 0.02 parts of dicumyl peroxide are mixed uniformly to obtain a premix; the premix and 50 parts of high-impact polystyrene, 26 parts of methyl acrylate-butadiene-styrene copolymer, and 4 parts of dibutyl phthalate are fully mixed uniformly through a high-speed mixer, and then formed and granulated at one time through a parallel twin-screw extruder to obtain a composite material based on modified heavy calcium carbonate.

[0040] Example 4

[0041] The composite material based on modified heavy calcium carbonate is prepared in the following specific steps:

[0042] 12 parts of the modified heavy calcium carbonate of Example 1, 1.5 parts of Clariant antistatic agent Hostastat FA 68V, 0.25 parts of antioxidant 1010 and 0.25 parts of antioxidant 168 compound, 0.3 parts of paraffin, 2 parts of phthalocyanine green and 0.03 parts of dicumyl peroxide are mixed uniformly to obtain a premix; the premix and 55 parts of high impact polystyrene, 35 parts of styrene-butadiene-styrene block copolymer and 5 parts of dioctyl phthalate are fully mixed uniformly by a high-speed mixer, and then formed and granulated by a parallel twin-screw extruder to obtain a composite material based on modified heavy calcium carbonate.

[0043] Comparative Example 1

[0044] The specific steps for preparing the composite material are as follows:

[0045] The remaining steps remained unchanged, except that the modified heavy calcium carbonate in Example 4 was replaced with heavy calcium carbonate without any treatment to prepare a composite material.

[0046] Performance Testing

[0047] The composite materials prepared in Examples 2-4 and Comparative Example 1 were subjected to the following performance tests, and the test results are shown in the following table:

[0048]

[0049] “-” means that the composite material is not flame retardant.

[0050] It can be seen from the above table that the composite material based on modified heavy calcium carbonate prepared in the embodiment of the present invention has excellent mechanical properties and flame retardant properties.

[0051] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0052] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A composite material based on modified heavy calcium carbonate, It is characterized in that The invention comprises the following raw materials in parts by weight: 45-55 parts of high impact polystyrene, 25-35 parts of toughening agent, 9-12 parts of modified heavy calcium carbonate, 3-5 parts of plasticizer, 0.1-0.5 parts of antioxidant, 0.5-1.5 parts of antistatic agent, 0.1-0.3 parts of lubricant, 1-2 parts of toner, and 0.01-0.03 parts of diisopropylbenzene peroxide; Wherein, the modified heavy calcium carbonate is prepared by the following steps: S1. Add guanidine melamine, triethylamine and DMSO into a flask, add diethyl (2-chloroethyl)phosphonate after stirring, react at 80° C. for 3 h, add deionized water, stir and let stand, take the organic phase, wash the organic phase with saturated brine, dry, filter and distill under reduced pressure to obtain intermediate 1; S2, add intermediate 1, 10-undecenoic acid, DMF and concentrated sulfuric acid into a flask, stir, react at 120°C for 8h, pour the reactant into an aqueous sodium bicarbonate solution after cooling, shake and let stand to separate the layers, wash the organic layer with an aqueous sodium bicarbonate solution and water until neutral, dry, and distill under reduced pressure to obtain intermediate 2; S3, add intermediate 2 and DMF into a flask, stir, heat to 80°C, add KH560, react at 80°C for 6h, cool, and distill under reduced pressure to obtain intermediate 3; S4. Ultrasonic disperse heavy calcium carbonate and deionized water for 30 minutes, pour into a flask, stir, and keep the temperature at 65°C; mix DMF and intermediate 3 evenly and add them into the flask, stir at 65°C for 10 hours, cool, filter, wash with anhydrous ethanol, and dry to obtain modified heavy calcium carbonate.

2. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The amount ratio of guanidine melamine, (2-chloroethyl) diethyl phosphonate, triethylamine and DMSO in step S1 is 10.1g:12g:8.3mL:120mL; the amount ratio of intermediate 1, 10-undecenoic acid, DMF and concentrated sulfuric acid in step S2 is 16.6g:33.3mL:110mL:3mL; the amount ratio of intermediate 2, KH560 and DMF in step S3 is 16.6g:5.7mL:120mL; the mass ratio of intermediate 3 to heavy calcium carbonate in step S4 is 3:

1.

3. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The toughening agent is one or more of styrene-butadiene-styrene block copolymer, ethylene-vinyl acetate copolymer, and methyl acrylate-butadiene-styrene copolymer.

4. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The plasticizer is one or more of di(2-ethylhexyl) phthalate, dibutyl phthalate, dioctyl phthalate and chlorinated paraffin.

5. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The antioxidant is one of antioxidant 1010, antioxidant 1076, antioxidant DLTP and antioxidant 168, or a combination of several of them.

6. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The antistatic agent is an ethoxylated alkylamine antistatic agent.

7. A composite material based on modified heavy calcium carbonate according to claim 1, It is characterized in that The lubricant is one or more of polyethylene wax, ethylene stearamide, ethylene bis stearamide and paraffin wax.

8. Use of a composite material based on modified heavy calcium carbonate according to claim 1 in the preparation of household appliances, automobiles and toys.

Citation Information

Patent Citations

  • Surface modification method for heavy calcium carbonate and method for preparing high polymer composite material through surface modification method

    CN107417968A

  • Modified heavy calcium carbonate, production method and application of modified heavy calcium carbonate in preparation of high-performance sealant

    CN117467287A