A composite modified halogen perovskite quantum dot and preparation method thereof

By generating in-situ halogen perovskite quantum dots in Schiff base metal-organic frameworks and reinforcing them with APTES, the problem of poor chemical stability is solved and higher stability and optoelectronic properties are achieved, making them suitable for industrial production.

CN118206982BActive Publication Date: 2024-10-11SHENZHEN LANGE SEA WHALE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410355341.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-11
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Halogen perovskite quantum dots have poor chemical stability under environmental conditions and are easily affected by water, light and temperature, which limits their application in fields such as light-emitting diodes, lasers, solar cells, etc., and existing synthesis methods are difficult for industrial production. Not suitable.

Method used

Schiff base metal-organic frameworks are used as carriers to generate halogen perovskite quantum dots in situ inside the carrier, and are reinforced by APTES hydrolysis to improve their stability while maintaining excellent optoelectronic properties.

Benefits of technology

Significantly improves the chemical stability of halogen perovskite quantum dots, controls the size distribution and uniformity of quantum dots, provides narrower bandwidth emission and higher photoluminescence quantum yield, reduces production costs and safety risks, Suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118206982B_ABST
    Figure CN118206982B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of nanomaterials, and specifically provides a composite modified halogen perovskite quantum dot and a preparation method thereof, wherein the composite modified halogen perovskite quantum dot comprises the following raw materials: Schiff base MOFs, lead halide, cesium halide, benign solvent, oleic acid, APTES, and recrystallization solvent. The Schiff base metal organic framework is used as a carrier to generate halogen perovskite quantum dots in situ inside the carrier, and further reinforced by APTES hydrolysis, thereby significantly improving the stability of the halogen perovskite quantum dots and maintaining excellent photoelectric properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a composite modified halogen perovskite quantum dot and a preparation method thereof. Background Art

[0002] Halogen perovskite quantum dots have attracted widespread attention for their ultra-high photoluminescence quantum yield, flexible and tunable emission wavelength, and narrowband emission characteristics, which have promoted their application in many fields such as light-emitting diodes, lasers, solar cells, photodetectors, and visible light communications. However, the main challenge facing halogen perovskite quantum dots is their poor chemical stability under environmental conditions. This is mainly because their low energy band position makes them extremely sensitive to water, light, and temperature. In addition, their high degree of ionic bonding leads to the susceptibility of ion exchange reactions and decomposition. These problems severely limit the practical application potential of halogen perovskite quantum dots and have become key issues that need to be urgently addressed in current research.

[0003] The synthesis of halogen perovskite quantum dots is mainly carried out through high-temperature hot injection method and room-temperature supersaturated recrystallization method; among them, the high-temperature hot injection method is to quickly inject the precursor solution into the hot solvent at high temperature, thereby promoting the rapid formation of perovskite crystals, and can obtain perovskite quantum dots with uniform size and shape in a very short time. However, the high-temperature hot injection method has high requirements for experimental conditions and poses certain safety risks to operators, and is not suitable for large-scale industrial production. The room-temperature supersaturated recrystallization method is a method of inducing crystal growth through a supersaturated solution under room temperature conditions, avoiding the safety risks of high-temperature heating, but slight changes in synthetic factors may affect the quality and uniformity of the crystals. In the batch production process, it is difficult to ensure that each batch of crystals has the same size and morphology. Therefore, it is urgent to explore a preparation method for highly stable composite modified halogen perovskite quantum dots. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a composite modified halogen perovskite quantum dots and a preparation method thereof, which utilizes a Schiff base metal organic framework as a carrier to in-situ generate halogen perovskite quantum dots inside the carrier, and further reinforces them through APTES hydrolysis, thereby significantly improving the stability of the halogen perovskite quantum dots and maintaining excellent photoelectric properties.

[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: The present invention proposes a composite modified halogen perovskite quantum dot, which includes the following raw materials: Schiff base MOFs, lead halide, cesium halide, benign solvent, oleic acid, APTES, and recrystallization solvent.

[0006] Preferably, the method for preparing the Schiff base MOFs comprises the following steps:

[0007] ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol. Continue to add 1 mol of salicylaldehyde, heat and reflux at 80℃ for 12 h, cool to room temperature and filter. Wash the filter cake three times with ethanol and place it in a vacuum drying oven. Dry it in vacuum at 60℃ for 12 h to obtain the Schiff base ligand. The reaction equation is as follows: Figure 1 As shown;

[0008] ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of the metal salt and 20-30 mmol of the regulator into 80 mL of DMF and mix well to obtain a precursor solution;

[0009] ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, heated in an oven at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs.

[0010] Preferably, the metal salt in step ② is any one of zirconium chloride, zirconium oxychloride, ferric chloride, ferric nitrate, europium chloride, europium nitrate, terbium chloride and terbium nitrate.

[0011] Preferably, the regulator in step ② is any one of benzoic acid, formic acid and acetic acid.

[0012] Preferably, the lead halide is any one of lead chloride and lead bromide.

[0013] Preferably, the cesium halide is any one of cesium chloride and cesium bromide.

[0014] Preferably, the benign solvent is any one of DMF and DMSO.

[0015] Preferably, the recrystallization solvent is any one of toluene and dichloromethane.

[0016] The present invention also provides a method for preparing composite modified halogen perovskite quantum dots, which specifically comprises the following steps:

[0017] S1. Weigh 50 mg of Schiff base MOFs and 2 mmol of lead halide into 40 mL of benign solvent, stir at 400 rpm for 4 h, then add 2 mmol of cesium halide, 2-3 mL of oleic acid, and 0.3-0.5 mL of APTES, and continue stirring for 15 min to obtain a precursor solution.

[0018] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 50-100 mL of recrystallization solvent, and the mixture was rapidly stirred at 800-1000 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0019] The beneficial effects achieved by the present invention are as follows:

[0020] The present invention uses Schiff base metal organic framework as a carrier to synthesize composite modified halogen perovskite quantum dots, which significantly improves the chemical stability of quantum dots. Among them, Schiff base has a strong metal ion coordination ability, which can effectively fix lead ions and reduce their damage by environmental factors. At the same time, synthesizing perovskite quantum dots in the structured environment of MOFs helps to control the size distribution and uniformity of quantum dots, thereby providing narrower bandwidth emission and higher photoluminescence quantum yield; and the added APTES can form a protective film on the surface of quantum dots through the silane group formed by its hydrolysis product. This protective film can not only effectively prevent the erosion of quantum dots by external moisture and oxygen, but also maintain excellent photoelectric properties while improving chemical stability. This synthesis method avoids high temperature conditions, which not only reduces production costs and safety risks, but also is expected to achieve mass production of quantum dots through stirring synthesis at room temperature, providing the possibility for the industrial production of perovskite quantum dots with improved stability and photoelectric efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 is the reaction equation for synthesizing Schiff base ligand;

[0023] Figure 2 This is a transmission electron microscopy image of the composite modified halogen perovskite quantum dots prepared in Example 1;

[0024] Figure 3 The XRD spectrum of the composite modified halogen perovskite quantum dots prepared in Example 1;

[0025] Figure 4 The fluorescence spectrum of the composite modified halogen perovskite quantum dots prepared in Example 1;

[0026] Figure 5The fluorescence stability spectra of the composite modified halogen perovskite quantum dots prepared in Examples 1-3 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below through examples and comparative examples, but this should not be understood as the scope of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention.

[0028] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples and comparative examples are purchased from commercial channels unless otherwise specified.

[0029] Example 1: This example proposes a composite modified halogen perovskite quantum dot, which includes the following raw materials: Schiff base MOFs, lead bromide, cesium bromide, DMF, oleic acid, APTES, and dichloromethane.

[0030] The preparation method of the Schiff base MOFs comprises the following steps:

[0031] ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol. Continue to add 1 mol of salicylaldehyde, heat and reflux at 80℃ for 12 h, cool to room temperature and filter. Wash the filter cake three times with ethanol and place it in a vacuum drying oven. Dry it in vacuum at 60℃ for 12 h to obtain the Schiff base ligand. The reaction equation is as follows: Figure 1 As shown;

[0032] ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of zirconium chloride and 20 mmol of benzoic acid, add them into 80 mL of DMF, mix well, and obtain a precursor solution;

[0033] ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, heated in an oven at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs.

[0034] This embodiment also provides a method for preparing composite modified halogen perovskite quantum dots, which specifically includes the following steps:

[0035] S1. Weigh 50 mg of Schiff base MOFs and add 2 mmol of lead bromide to 40 mL of DMF, stir at 400 rpm for 4 h, then add 2 mmol of cesium bromide, 2 mL of oleic acid, and 0.4 mL of APTES, and continue stirring for 15 min to obtain a precursor solution.

[0036] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 100 mL of dichloromethane, and the mixture was rapidly stirred at 800 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0037] Example 2: This example proposes a composite modified halogen perovskite quantum dot, which includes the following raw materials: Schiff base MOFs, lead chloride, cesium chloride, DMSO, oleic acid, APTES, and toluene.

[0038] The preparation method of the Schiff base MOFs comprises the following steps:

[0039] ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol. Continue to add 1 mol of salicylaldehyde, heat and reflux at 80℃ for 12 h, cool to room temperature and filter. Wash the filter cake three times with ethanol and place it in a vacuum drying oven. Dry it in vacuum at 60℃ for 12 h to obtain the Schiff base ligand. The reaction equation is as follows: Figure 1 As shown;

[0040] ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of ferric chloride and 30 mmol of formic acid, add them into 80 mL of DMF, mix well, and obtain a precursor solution;

[0041] ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, heated in an oven at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs.

[0042] This embodiment also provides a method for preparing composite modified halogen perovskite quantum dots, which specifically includes the following steps:

[0043] S1. Weigh 50 mg of Schiff base MOFs and add 2 mmol of lead chloride to 40 mL of DMSO, stir at 400 rpm for 4 h, then add 2 mmol of cesium chloride, 3 mL of oleic acid, and 0.3 mL of APTES, and continue stirring for 15 min to obtain a precursor solution.

[0044] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 50 mL of toluene, and the mixture was rapidly stirred at 1000 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0045] Example 3: This example proposes a composite modified halogen perovskite quantum dot, which includes the following raw materials: Schiff base MOFs, lead bromide, cesium bromide, DMF, oleic acid, APTES, and toluene.

[0046] The preparation method of the Schiff base MOFs comprises the following steps:

[0047] ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol. Continue to add 1 mol of salicylaldehyde, heat and reflux at 80℃ for 12 h, cool to room temperature and filter. Wash the filter cake three times with ethanol and place it in a vacuum drying oven. Dry it in vacuum at 60℃ for 12 h to obtain the Schiff base ligand. The reaction equation is as follows: Figure 1 As shown;

[0048] ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of europium chloride and 25 mmol of acetic acid, add them into 80 mL of DMF, mix well, and obtain a precursor solution;

[0049] ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, heated in an oven at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs.

[0050] This embodiment also provides a method for preparing composite modified halogen perovskite quantum dots, which specifically includes the following steps:

[0051] S1. Weigh 50 mg of Schiff base MOFs and add 2 mmol of lead bromide to 40 mL of DMF, stir at 400 rpm for 4 h, then add 2 mmol of cesium bromide, 2.5 mL of oleic acid, and 0.5 mL of APTES, and continue stirring for 15 min to obtain a precursor solution.

[0052] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 80 mL of toluene, and the mixture was rapidly stirred at 900 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane for three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0053] Comparative Example 1: The comparative example proposes a composite modified halogen perovskite quantum dot, which differs from Example 1 only in that Schiff base MOFs are not added. The composite modified halogen perovskite quantum dot includes the following raw materials: lead bromide, cesium bromide, DMF, oleic acid, APTES, and dichloromethane.

[0054] This comparative example also proposes a method for preparing composite modified halogen perovskite quantum dots, which specifically comprises the following steps:

[0055] S1. Weigh 2 mmol lead bromide and add it to 40 mL DMF. Stir at 400 rpm for 4 h. Then add 2 mmol cesium bromide, 2 mL oleic acid, and 0.4 mL APTES. Stir for 15 min to obtain a precursor solution.

[0056] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 100 mL of dichloromethane, and the mixture was rapidly stirred at 800 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0057] Comparative Example 2: This comparative example proposes a composite modified halogen perovskite quantum dot, which differs from Example 1 only in that the ligand for synthesizing the MOFs material is 2-aminoterephthalic acid, and the Schiff base ligand is not synthesized. The remaining components, component contents, and experimental steps are the same as those in Example 1; the composite modified halogen perovskite quantum dots include the following raw materials: MOFs, lead bromide, cesium bromide, DMF, oleic acid, APTES, and dichloromethane.

[0058] The preparation method of MOFs comprises the following steps:

[0059] ① Weigh 10 mmol of 2-aminoterephthalic acid, 10 mmol of zirconium chloride and 20 mmol of benzoic acid, add them into 80 mL of DMF, mix well, and obtain a precursor solution;

[0060] ② Place the precursor solution prepared in step ① in a reactor lined with polytetrafluoroethylene, heat it in an oven at 120°C for 12 h, cool it to room temperature, wash it alternately with DMF and ethanol three times, place it in a vacuum drying oven at 60°C for 12 h, and obtain MOFs.

[0061] This embodiment also provides a method for preparing composite modified halogen perovskite quantum dots, which specifically includes the following steps:

[0062] S1. Weigh 50 mg MOFs and 2 mmol lead bromide into 40 mL DMF, stir at 400 rpm for 4 h, then add 2 mmol cesium bromide, 2 mL oleic acid, and 0.4 mL APTES, and continue stirring for 15 min to obtain a precursor solution.

[0063] S2. Under air atmosphere, the precursor solution prepared in step S1 was quickly added into 100 mL of dichloromethane, and the mixture was rapidly stirred at 800 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed alternately with n-hexane and dichloromethane three times, and the precipitate was placed in a vacuum drying oven and dried at 40 °C for 24 h to obtain composite modified halogen perovskite quantum dots.

[0064] Comparative Example 3: This comparative example proposes a composite modified halogen perovskite quantum dot, which differs from Example 1 only in that APTES is not added, and the remaining components, component contents, and experimental steps are the same as those in Example 1.

[0065] Experimental Example 1: The microscopic morphology of the composite modified halogen perovskite quantum dots prepared in Example 1 was observed using a transmission electron microscope. The structural characteristics of the composite modified halogen perovskite quantum dots prepared in Example 1 were analyzed using an X-ray diffractometer.

[0066] Figure 2 This is a transmission electron micrograph of the composite modified halogen perovskite quantum dots prepared in Example 1. As shown in the figure, perovskite quantum dots with smaller particle sizes are distributed in the composite material. Due to the hydrolysis and condensation of the silane coupling agent APTES, the composite material undergoes a certain aggregation, thereby improving stability. Figure 3 This is the XRD spectrum of the composite modified halogen perovskite quantum dots prepared in Example 1. As shown in the figure, the diffraction peak of the composite material is consistent with the cubic perovskite crystal structure and contains the diffraction peak of the MOFs structure.

[0067] Experimental Example 2: Fluorescence Performance Test

[0068] The composite modified halogen perovskite quantum dots prepared in Example 1 were dispersed in water to prepare a 10 mg / L detection solution, and its fluorescence spectrum was measured using a fluorescence photometer. During the experiment, the fluorescence detection conditions of the instrument were set as follows: the excitation wavelength was 365 nm, the slit widths of the excitation wavelength and the emission wavelength were both 5 nm, the photomultiplier tube voltage was 550 V, and the recorded emission wavelength range was 400-600 nm.

[0069] Figure 4 This is the fluorescence spectrum of the composite modified halogen perovskite quantum dots prepared in Example 1. As shown in the figure, under the excitation of 365nm wavelength, the composite modified halogen perovskite quantum dots has a maximum emission wavelength at 512nm, a high fluorescence intensity, and a narrow maximum half-peak width of about 30nm, a high fluorescence color purity, and a high quantum efficiency.

[0070] Experimental Example 3: Fluorescence stability test

[0071] The composite modified halogen perovskite quantum dots prepared in Examples 1-3 and Comparative Examples 1-3 were respectively dispersed in water to prepare a 10 mg / L quantum dot solution, and the fluorescence value was measured every five days.

[0072] Figure 5 The fluorescence stability spectra of the composite modified halogen perovskite quantum dots prepared in Examples 1-3 and Comparative Examples 1 to 3 are as shown in the figure. The fluorescence of the perovskite quantum dots prepared in Examples 1-3 does not change much in polar solvent water within 50 days, while the perovskite quantum dots prepared in Comparative Example 1 have no protection from the MOFs shell and their fluorescence value decreases rapidly, that is, the structure of the perovskite quantum dots is destroyed. The fluorescence of the perovskite quantum dots prepared in Comparative Examples 1-2 also decreases to a certain extent, indicating that the Schiff base binding sites in the MOFs material and the silicon structure of APTES hydrolysis condensation can improve the structural stability of the halogen perovskite quantum dots.

[0073] The present invention and its implementation methods are described above, and such description is not restrictive, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the purpose of the invention, they can design methods and embodiments similar to the technical solution without creativity, which should all fall within the protection scope of the present invention.

Claims

1. A composite modified halogen perovskite quantum dot, characterized in that: The preparation process of the composite modified halogen perovskite quantum dots includes the following raw materials: Schiff base MOFs, lead halide, cesium halide, benign solvent, oleic acid, APTES, and recrystallization solvent; The preparation method of the Schiff base MOFs comprises the following steps: ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol, then add 1 mol of salicylaldehyde, heat and reflux at 80°C for 12 h, cool to room temperature and filter, wash the filter cake three times with ethanol and place it in a vacuum drying oven, vacuum dry it at 60°C for 12 h to obtain the Schiff base ligand; ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of the metal salt and 20-30 mmol of the regulator into 80 mL of DMF and mix well to obtain a precursor solution; ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, placed in an oven and heated at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs; The preparation method of the composite modified halogen perovskite quantum dots comprises the following steps: S1. Weigh 50 mg of Schiff base MOFs and 2 mmol of lead halide into 40 mL of benign solvent, stir at 400 rpm for 4 h, then add 2 mmol of cesium halide, 2-3 mL of oleic acid, and 0.3-0.5 mL of APTES, and continue stirring for 15 min to obtain a precursor solution. S2. In an air atmosphere, the precursor solution prepared in step S1 was quickly added to 50-100 mL of a recrystallization solvent, and the mixture was rapidly stirred at 800-1000 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed three times with n-hexane and dichloromethane alternately, and the precipitate was placed in a vacuum drying oven and dried at 40° C. for 24 h to obtain composite modified halogen perovskite quantum dots. In step ②, the metal salt is any one of zirconium chloride, zirconium oxychloride, ferric chloride, ferric nitrate, europium chloride, europium nitrate, terbium chloride, and terbium nitrate; In the step ②, the regulator is any one of benzoic acid, formic acid and acetic acid.

2. The composite modified halogen perovskite quantum dot according to claim 1, characterized in that: The lead halide is any one of lead chloride and lead bromide.

3. The composite modified halogen perovskite quantum dot according to claim 2, characterized in that: The cesium halide is any one of cesium chloride and cesium bromide.

4. The composite modified halogen perovskite quantum dot according to claim 3, characterized in that: The benign solvent is any one of DMF and DMSO.

5. The composite modified halogen perovskite quantum dot according to claim 4, characterized in that: The recrystallization solvent is any one of toluene and dichloromethane.

6. A method for preparing the composite modified halogen perovskite quantum dots according to any one of claims 1 to 5, characterized in that: The specific steps include: S1. Weigh 50 mg of Schiff base MOFs and 2 mmol of lead halide into 40 mL of benign solvent, stir at 400 rpm for 4 h, then add 2 mmol of cesium halide, 2-3 mL of oleic acid, and 0.3-0.5 mL of APTES, and continue stirring for 15 min to obtain a precursor solution. S2. In an air atmosphere, the precursor solution prepared in step S1 was quickly added to 50-100 mL of a recrystallization solvent, and the mixture was rapidly stirred at 800-1000 rpm for 30 min to completely hydrolyze APTES. The precipitate was washed three times with n-hexane and dichloromethane alternately, and the precipitate was placed in a vacuum drying oven and dried at 40° C. for 24 h to obtain composite modified halogen perovskite quantum dots. The method for preparing Schiff base MOFs in step S1 comprises the following steps: ① Weigh 1 mol of 2-aminoterephthalic acid and add it to 50 mL of ethanol, then add 1 mol of salicylaldehyde, heat and reflux at 80°C for 12 h, cool to room temperature and filter, wash the filter cake three times with ethanol and place it in a vacuum drying oven, vacuum dry it at 60°C for 12 h to obtain the Schiff base ligand; ② Weigh 10 mmol of the Schiff base ligand prepared in step ①, 10 mmol of the metal salt and 20-30 mmol of the regulator into 80 mL of DMF and mix well to obtain a precursor solution; ③ The precursor solution prepared in step ② was placed in a reactor lined with polytetrafluoroethylene, heated in an oven at 120°C for 12 h, cooled to room temperature, washed alternately with DMF and ethanol three times, and placed in a vacuum drying oven at 60°C for 12 h to obtain Schiff base MOFs.