Bionic toughening structure of pearl layer between layers of high-speed impact-resistant and wave-transparent composite materials and its simplified preparation process
By constructing a low-dielectric interlayer naphthalene bionic toughening structure, using the soft-hard alternating structure of aerogel and resin matrix, the problems of layered failure and dielectric properties of composite materials under high-speed impact are solved, and high Improved impact resistance and wave transmission performance.
Patent Information
- Application Number
- CN202410067663.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-01-17
AI Technical Summary
Composite materials are prone to stratification failure under high-speed impact, which is difficult to provide sufficient stiffness and wave transmission performance, and requires low dielectric properties. It is difficult for the prior art to simultaneously improve the resistance to penetration and depression resistance.
Using low-dielectric sheet materials and resin matrix to construct interlayer naphthalene bionic toughening structures with natural shell structures, the soft-hard alternating structures of aerogel and resin matrix are formed through directional refrigeration technology to enhance interlayer performance and suppress Crack Propagation.
The composite material has achieved low dielectric, high wave transmission, low deformation and high impact resistance, effectively suppressing stratified failure and non-penetrating damage, and improving the overall mechanical and wave transmission performance of the material.
Smart Images

Figure CN118219637B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a nacre bionic toughening structure between layers of a high-speed impact resistant and wave-transmitting composite material and a simplified preparation process thereof. Background Art
[0002] Composite materials are the main material of radar antenna covers. While providing an electromagnetic window for the antenna system, they also need to protect it from damage from the harsh natural environment and high-speed impacts from unknown objects outside the surface. The increasingly complex battlefield environment has put forward more stringent protection performance requirements for composite materials. Not only are they required to provide excellent wave transmission performance and maintain the overall mechanical properties of the structure in a complex and changeable battlefield environment, but they are also required to minimize their own weight to provide better maneuverability. As a new generation of protective materials, reinforced resin-based composite materials such as ultra-high molecular weight polyethylene (UHMWPE) fibers, poly(p-phenylene benzobisoxazole) fibers and aramid fibers have been a research hotspot in this field in recent years, and have also been widely used. Fiber-reinforced resin-based composite materials have excellent impact resistance and protection properties, and the density is mostly 3g / cm 3 Compared with traditional metal protective materials, the following is significantly reduced, thus accelerating the development of lightweight and high mobility of weapons and equipment. However, in practical applications, impact can easily lead to delamination of fiber-reinforced resin-based composite materials and large back protrusions. Although it can effectively protect against penetrating damage, it can easily cause material structural failure caused by non-penetrating damage, and it is difficult to provide the stiffness required by structural materials. To solve these problems, the commonly used method is to increase the bonding strength between composite material layers.
[0003] To resist penetration damage, the composite material needs to have a large in-plane tensile deformation under the action of out-of-plane loads, so as to give full play to the axial tensile properties of the fiber; while to resist non-penetrating damage, it is hoped that the composite material has a high in-plane stiffness to reduce the depression deformation. Traditional research based on energy dissipation mechanism believes that penetration resistance and depression resistance are a pair of contradictory properties. For special application environments, such as radar antenna covers, it is also an important issue that cannot be avoided that the material should have low dielectric properties, which requires that while reinforcing the composite material, materials and structures with high dielectric properties cannot be introduced.
[0004] The key to the above problems lies in the interface of the composite material. Therefore, seeking an interface toughening method with excellent fracture toughness, low plastic deformation, low dielectric and high wave transmittance is an urgent problem to be solved in the current application of composite materials in the field of radar antenna covers. Summary of the invention
[0005] The present invention overcomes the shortcomings of the prior art and provides a nacre bionic toughening structure between layers of a high-speed impact-resistant wave-transmitting composite material. The interlayer toughening structure has the performance characteristics of low dielectric and high crack arrest; the preparation process is simple and convenient. Compared with the traditional single-component interlayer toughening structure, the structurally toughened composite protective material of the present invention has the advantages of low deformation, high impact resistance, low dielectric, high wave transmission, etc.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a nacre bionic toughening structure between layers of high-speed impact resistant wave-transmitting composite materials, comprising an upper composite material, a lower composite material, and an interlayer nacre bionic toughening structure constructed between the upper and lower composite material layers by a low-dielectric sheet material and a resin matrix, which has the characteristics of preventing crack extension, improving interlayer performance, and having a low dielectric high-performance soft-hard alternating nacre structure similar to that of shells in nature;
[0007] The upper composite material is selected from one of a fiber-reinforced resin-based composite material, a foam material and a honeycomb material;
[0008] The lower layer composite material is selected from one of a fiber-reinforced resin-based composite material, a foam material and a honeycomb material;
[0009] The interlayer nacre bionic toughening structure is an aerogel completely filled with resin; it uses directional freezing technology to assemble the α-ZrP sheets into a continuous network structure with a specific orientation direction, and further fills the inside of the network structure with a resin matrix, and finally the resin matrix constitutes a soft layer and the oriented α-ZrP aerogel wall constitutes a hard layer, thereby constructing a soft-hard alternating nacre-like structure between the composite material layers;
[0010] The resin soft layer can bond the aerogel into a whole and maintain a certain shape, transfer interlayer stress, and protect the aerogel from external erosion and damage; the low dielectric oriented α-ZrP hard layer filled between the composite material layers in the form of aerogel has the function of improving the mechanical properties and wave transmission performance of the interlayer toughening structure. In addition, when the overall structure is impacted, the cracks are deflected, differentiated, and terminated, thereby hindering the expansion of the main cracks between the layers, thereby effectively inhibiting stratification.
[0011] The interlayer pearl layer bionic toughening structure is applicable to the interlayers of the same or different fiber-reinforced resin composite materials, the interlayers of foams and honeycombs with discontinuous characteristics, and the interlayers between them and fiber-reinforced resin composite materials.
[0012] As a further improvement of the technical solution of the present invention, the aerogel is an aerogel obtained by directional freezing of an aqueous dispersion system of α-ZrP nanosheets and cellulose after in-situ exfoliation, and has a directional orientation in a vertical direction to a horizontal direction, uniform wall thickness, and uniform pore distribution; cellulose serves as a structural reinforcement framework of the oriented α-ZrP aerogel, and can enhance the structure of the oriented α-ZrP aerogel;
[0013] The in-situ exfoliated α-ZrP nanosheets are exfoliated by using small molecule substances containing amino groups as exfoliants and utilizing ultrasound-assisted exfoliation technology to exfoliate the original α-ZrP nanosheets, and α-ZrP nanosheets of different two-dimensional sizes and thicknesses are finally obtained by controlling the exfoliation time and ultrasound power;
[0014] The cellulose is selected from at least one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose and bacterial cellulose.
[0015] As a further improvement of the technical solution of the present invention, the stripping agent is selected from at least one of triethanolamine, ethylenediamine and lysine.
[0016] As a further improvement of the technical solution of the present invention, the resin matrix is a thermosetting resin system obtained by uniformly mixing a thermosetting resin, a curing agent and a reaction aid; the thermosetting resin is selected from at least one of an epoxy resin, an unsaturated polyester resin and a phenolic resin; the reaction aid includes any one or more mixtures of an initiator, a promoter and a catalyst.
[0017] As a further improvement of the technical solution of the present invention, in the water dispersion system of α-ZrP nanosheets and cellulose for preparing aerogel, the mass ratio of α-ZrP to cellulose is 10-5:2-1.
[0018] As a further improvement of the technical solution of the present invention, the α-ZrP nanosheet is a nanometer-level two-dimensional sheet material, the two-dimensional sheet size is 300-1700nm, and the sheet thickness is 30-100nm; the thickness of the α-ZrP aerogel is 0.1-0.4mm, and the surface density is 20-100g / m 2 .
[0019] As a further improvement of the technical solution of the present invention, the thickness of the interlayer pearl layer bionic toughening structure is 0.1-0.4 mm, the dielectric constant value is 2.45-2.72, the loss tangent value is 0.028-0.042, the bending strength is 100-130 MPa, the maximum bending strain is 4-6%, and the type I critical energy release rate is 1.02-1.58 kJ / m 2 ; Type I critical energy release rate of bonding interface is 0.7~1.2kJ / m 2 The critical energy release rate of bonding interface type II is 3.0~3.8kJ / m2 , the interlaminar shear strength reaches 55~75MPa.
[0020] The present invention also provides a simplified preparation process of the nacre bionic toughening structure between the layers of the high-speed impact wave-transmitting composite material, comprising the following steps:
[0021] (1) uniformly dispersing α-ZrP powder in water, adding a certain amount of stripping agent, and stirring until the dispersion is uniform and free of precipitation to obtain an intercalated α-ZrP dispersion; transferring the dispersion to a cell disruptor, controlling the ultrasonic power and ultrasonic time, and obtaining α-ZrP dispersions with different stripping degrees;
[0022] (2) adding cellulose to the α-ZrP dispersion obtained in step (1) after stripping and completely dissolving the cellulose to obtain a uniform water dispersion system; pouring the obtained uniform water dispersion system into a copper bottom mold parallel to the ground, so that the liquid nitrogen covers the copper bottom, and after the water dispersion system is completely frozen, transferring the mold to a freeze dryer, taking it out and demolding it after drying, to obtain an α-ZrP aerogel;
[0023] (3) mixing a thermosetting resin and a curing agent, mechanically stirring until the color is uniform and without stratification, then adding a reaction aid thereto, mechanically stirring until the color is uniform; then vacuum degassing in an oven until no bubbles are generated to obtain a resin glue solution;
[0024] (4) impregnating the α-ZrP aerogel prepared in step (2) into the resin glue prepared in step (3), evacuating the air so that the resin completely fills the aerogel, raising the temperature to perform pre-curing when there are no bubbles, and taking out the aerogel after the resin matrix is gelled to obtain a pre-cured body of the interlayer nacre bionic toughening structure;
[0025] (5) placing the precured body of the interlayer pearl layer bionic toughening structure obtained in step (4) between the layers of two composite materials to be bonded, and using liquid molding or autoclave technology to solidify the interlayer toughening phase and the two composite materials as a whole, thereby obtaining a pearl layer bionic toughening structure between the layers of a high-speed impact-resistant and wave-transparent composite material.
[0026] As a further improvement of the technical solution of the present invention, in step (1), the power of the cell disruptor is 150 to 300 W, and the ultrasonic time is 3 to 15 min; in step (2), the temperature of the liquid nitrogen is -196°C; the vacuum degree of the freeze-drying is -0.05 to -0.09 MPa, the temperature is -65 to -45°C, and the time is 36 to 48 h.
[0027] As a further improvement of the technical solution of the present invention, in step (4), the vacuum degree of vacuuming is -0.09 MPa, the vacuuming rate is 2 L / min, the temperature is 60 to 80°C, and the vacuuming time is 0.5 to 1 h.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The interlayer toughening method of the present invention has high interlayer performance of composite materials, can improve the critical energy release rate of the whole material, effectively inhibit interlayer delamination failure and penetrating damage and non-penetrating damage caused by out-of-plane impact on the composite material, and also has high wave transmission performance. It can be applied to fields with high requirements on the impact resistance and wave transmission performance of composite materials, such as meteorological radar antenna covers, vehicle-mounted antenna covers, aircraft shells, etc.
[0030] (2) The interlayer toughening structure of the present invention, the thermosetting resin system can bond the aerogel into a whole and maintain a certain shape, transfer interlayer stress, protect the aerogel from external erosion and damage, etc.; cellulose serves as a reinforcing frame of the α-ZrP aerogel structure, which plays a role in strengthening the α-ZrP aerogel structure; at the same time, α-ZrP, as a low dielectric material, is filled in the interlayer of the composite material in the form of aerogel, which can play a role in improving the interlayer phase mechanics and wave transmission performance; when the overall structure is subjected to an out-of-plane impact, the crack propagates between the layers, and when it reaches the aerogel wall, the aerogel wall composed of α-ZrP sheets slips, pulls out, and breaks. These methods can reduce and eliminate the stress concentration generated at the crack propagation tip, consume a lot of energy, and hinder the propagation of the main crack between the layers by causing the crack to deflect, differentiate, and terminate, thereby effectively inhibiting delamination.
[0031] (3) The modulus of the α-ZrP layer is quite different from that of the resin matrix. Such an alternating arrangement with a large modulus difference can also effectively prevent cracks.
[0032] (4) Aerogel can expand the interlayer space, thereby increasing the glue content between the composite layers, making it more difficult for cracks to extend to the relatively fragile interface, thereby effectively improving the overall performance and anti-delamination performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of a nacre bionic toughening structure between layers of a high-speed impact resistant and wave-transmitting composite material of the present invention.
[0034] Figure 2 This is a SEM photograph of the nacre bionic toughening structure between the composite materials prepared in Example 1 after high-speed impact.
[0035] The following are marked in the figure:
[0036] 1-upper composite material, 2-interlayer nacre bionic toughening structure, 3-lower composite material, 4-α-ZrP aerogel, 5-resin matrix phase. DETAILED DESCRIPTION
[0037] The present invention is further described below in conjunction with specific embodiments.
[0038] Example 1
[0039] A bionic toughened pearl layer structure between glass fiber cloth reinforced epoxy resin-based composite materials and ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite materials with high-speed impact resistance and wave-transmitting properties, wherein the simplified preparation process comprises the following steps:
[0040] (1) Weigh 20 g of E-51 epoxy resin, add 15.8 g of anhydride curing agent hexahydrophthalic anhydride (HHPA) and 0.06 g of accelerator 2.4.6-tris(dimethylaminomethyl)phenol (DMP-30), mix well and degas under vacuum at 50° C. until no bubbles are generated, to obtain epoxy resin glue;
[0041] (2) 1.43 g of α-ZrP powder was uniformly dispersed in 150 ml of deionized water, and 1.51 g of exfoliating agent triethanolamine was added at a molar ratio of 2:1, and stirred until the dispersion was uniform and free of precipitation to obtain an intercalated α-ZrP dispersion; the dispersion was transferred to a cell disruptor and ultrasonicated at a power of 300 W for 9 min to obtain an exfoliated α-ZrP nanosheet dispersion, wherein the average size of the α-ZrP two-dimensional sheet was 600 nm and the average sheet thickness was 40 nm;
[0042] (3) Add 0.4 g of hydroxyethyl cellulose to the prepared in-situ exfoliated α-ZrP sheet dispersion until the hydroxyethyl cellulose is completely dissolved to obtain a uniform α-ZrP / cellulose aqueous dispersion system, which is then poured into a copper-bottomed mold parallel to the ground so that the liquid nitrogen covers the copper bottom. After the aqueous dispersion system is completely frozen, the mold is transferred to a freeze dryer with the parameters set to a cold trap temperature of -65°C, a vacuum degree of -0.05 MPa, and freeze drying for 36 hours; after drying, the mold is removed and demolded to obtain an α-ZrP aerogel with a thickness of 0.1 mm and an area density of 40 g / m 2 ;
[0043] (4) impregnating the α-ZrP aerogel prepared in step (3) into the epoxy resin glue prepared in step (1), evacuating at 70° C. to completely fill the aerogel with the resin, with a evacuation rate of 2 L / min for 0.5 h, raising the temperature to 100° C. for pre-curing when there are no bubbles, and taking it out after the epoxy resin matrix is gelled to obtain a pre-cured body of the interlayer toughening phase;
[0044] (5) A hard single-sided mold is used, a mold release agent is applied on the surface of the mold, and then a glass fiber cloth reinforced epoxy resin-based composite material, a precured body of the interlayer toughening phase obtained in step (4), and an ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material are laid in sequence, and the material system is sealed on the mold with a polytetrafluoroethylene film; then a vacuum pump is connected, and the mold is transferred to a heating table, and cured at 140° C. and 1 atmosphere for 3 hours to obtain a high-speed impact-resistant and wave-transparent interlayer pearl layer bionic toughening structure of the glass fiber cloth reinforced epoxy resin-based composite material and the ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material.
[0045] The preparation process of glass fiber cloth reinforced epoxy resin-based composite material and ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material for bonding is as follows:
[0046] (I) Preparation of epoxy resin glue: 150 g of E-51 epoxy resin was weighed, 118.5 g of HHPA and 0.7 g of DMP-30 were added thereto, and the mixture was degassed in a vacuum at 50° C. until no bubbles were generated, thereby obtaining epoxy resin glue.
[0047] (II) Preparation of glass fiber cloth reinforced epoxy resin-based composite materials: The mold is coated with a release agent, and the glass fiber cloth is laid in an orthogonal laying manner. After each layer is laid, it is soaked with the epoxy resin glue prepared in step (I). After laying 10 layers, the mold is wrapped with a polytetrafluoroethylene film and hot-pressed at 100° C. in a hot press for 45 minutes; then the temperature is raised to 140° C. and hot-pressed for 2 hours to obtain a glass fiber cloth reinforced epoxy resin-based composite material.
[0048] (III) Preparation of ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite materials: The mold is coated with a release agent, and ultra-high molecular weight polyethylene fiber cloth is laid in an orthogonal laying manner. After each layer is laid, it is soaked with the epoxy resin glue prepared in step (I). After laying 10 layers, the mold is wrapped with a polytetrafluoroethylene film and hot-pressed at 100°C in a hot press for 45 minutes; then the temperature is raised to 140°C and hot-pressed for 2 hours to obtain an ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material.
[0049] Figure 2 This is a SEM photo of the bionic toughening structure of the pearl layer between the composite materials prepared in Example 1 after high-speed impact. Figure 2 It can be seen that the aerogel stands between the layers in a cross-linked network structure with a specific orientation perpendicular to the horizontal direction. Between the aerogel walls, there is residual resin matrix that is broken due to stress concentration; the aerogel walls are missing to varying degrees due to crack expansion. The appearance of these phenomena indicates that the interlayer toughness has been improved.
[0050] Comparative Example 1
[0051] A pure epoxy resin toughening structure between layers of a glass fiber cloth reinforced epoxy resin-based composite material and an ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material, wherein the preparation process comprises the following steps:
[0052] (1) Same as (1) of Example 1;
[0053] (2) A hard single-sided mold is used, a mold release agent is applied on the surface of the mold, a glass fiber cloth reinforced epoxy resin-based composite material is laid, a certain thickness of the epoxy resin glue obtained in step (1) is applied thereon, and then an ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material is laid thereon, and the material system is sealed on the mold with a polytetrafluoroethylene film; then a vacuum pump is connected, the mold is transferred to a heating table, and cured at 140° C. and 1 atmosphere for 3 hours to obtain a pure epoxy toughened structure between the glass fiber cloth reinforced epoxy resin-based composite material and the ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material layers.
[0054] The preparation process of the glass fiber cloth reinforced epoxy resin-based composite material and the ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material used for bonding is exactly the same as that in Example 1.
[0055] Comparative Example 2
[0056] A glass fiber cloth reinforced epoxy resin-based composite material and an ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material interlayer α-ZrP powder / epoxy composite toughening structure, the preparation process of which comprises the following steps:
[0057] (1) Weigh 20 g of E-51 epoxy resin, add 15.8 g of HHPA and 0.06 g of DMP-30, mix well, add the same amount of α-ZrP powder as in Example 1, mix well, and degas under vacuum at 50° C. until no bubbles are generated, to obtain α-ZrP powder / epoxy composite resin glue;
[0058] (2) The same as (2) of Comparative Example 1, except that a certain thickness of α-ZrP powder / epoxy resin glue obtained in step (1) is brushed on the surface of the glass fiber cloth reinforced epoxy resin-based composite material.
[0059] The preparation process of the glass fiber cloth reinforced epoxy resin-based composite material and the ultra-high molecular weight polyethylene fiber cloth reinforced epoxy resin-based composite material used for bonding is exactly the same as that in Example 1.
[0060] Example 2
[0061] A bionic toughened pearl layer structure of glass fiber cloth reinforced epoxy resin-based composite material and polyvinyl chloride closed-cell foam board that resists high-speed impact and transmits waves, and a simplified preparation process thereof comprises the following steps:
[0062] (1) Weigh 30 g of E-51 epoxy resin, add 23.7 g of HHPA and 0.09 g of DMP-30, mix well, and vacuum degas at 50° C. until no bubbles are generated to obtain epoxy resin glue;
[0063] (2) 2.15 g of α-ZrP powder was uniformly dispersed in 150 ml of deionized water, and 2.27 g of triethanolamine was added at a molar ratio of 2:1, and stirred until the dispersion was uniform and free of precipitation to obtain an intercalated α-ZrP dispersion; the dispersion was transferred to a cell disruptor and ultrasonicated at a power of 300 W for 6 min to obtain an exfoliated α-ZrP nanosheet dispersion, wherein the average size of the α-ZrP two-dimensional sheet was 1000 nm and the average sheet thickness was 60 nm;
[0064] (3) Same as (3) of Example 1; the thickness of the obtained α-ZrP aerogel is 0.2 mm and the surface density is 80 g / m 2 ;
[0065] (4) Same as (4) of Example 1;
[0066] (5) The same as (5) of Example 1, except that the cleaned polyvinyl chloride closed-cell foam board is used instead of the ultra-high molecular weight polyethylene fiber cloth to reinforce the epoxy resin-based composite material.
[0067] The preparation process of glass fiber cloth reinforced epoxy resin matrix composite material for bonding is as follows:
[0068] (I) Same as (I) of Example 1;
[0069] (II) Same as (II) in Example 1;
[0070] (III) Treatment of PVC closed-cell foam board products: Clean the surface dirt of the foam board with deionized water, and then wipe it with ethanol several times.
[0071] Comparative Example 3
[0072] A glass fiber cloth reinforced epoxy resin-based composite material and a pure epoxy resin toughened structure between polyvinyl chloride closed-cell foam boards, the preparation process of which comprises the following steps:
[0073] (1) Same as (1) of Example 2;
[0074] (2) A hard single-sided mold is used, a mold release agent is applied on the surface, a glass fiber cloth reinforced epoxy resin-based composite material is laid, a certain thickness of the epoxy resin glue obtained in step (1) is brushed thereon, and then a cleaned polyvinyl chloride closed-cell foam board is laid thereon, and the material system is sealed on the mold with a polytetrafluoroethylene film; then a vacuum pump is connected, and the mold is transferred to a heating table, and cured at 140° C. and 1 atmosphere for 3 hours to obtain a pure epoxy toughened structure between the glass fiber cloth reinforced epoxy resin-based composite material and the polyvinyl chloride closed-cell foam board.
[0075] The preparation process of the glass fiber cloth reinforced epoxy resin-based composite material used for bonding and the cleaning process of the polyvinyl chloride closed-cell foam board are exactly the same as those in Example 2.
[0076] Comparative Example 4
[0077] A glass fiber cloth reinforced epoxy resin-based composite material and an α-ZrP powder / epoxy composite toughening structure between layers of a polyvinyl chloride closed-cell foam board, the preparation process of which comprises the following steps:
[0078] (1) Weigh 30 g of E-51 epoxy resin, add 23.7 g of HHPA and 0.09 g of DMP-30, add the same amount of α-ZrP powder as in Example 2 after mixing, and degas under vacuum at 50° C. until no bubbles are generated to obtain α-ZrP powder / epoxy composite resin glue;
[0079] (2) The same as (2) of Comparative Example 3, except that a certain thickness of α-ZrP powder / epoxy resin glue obtained in step (1) is brushed on the surface of the glass fiber cloth reinforced epoxy resin-based composite material.
[0080] The preparation process of the glass fiber cloth reinforced epoxy resin-based composite material used for bonding and the cleaning process of the polyvinyl chloride closed-cell foam board are exactly the same as those in Example 2.
[0081] Table 1 shows the properties of Examples 1-2 and Comparative Examples 1-4. The dielectric constant and dielectric loss tangent of the interlayer toughening structure in the Examples and Comparative Examples were measured by the coaxial method; the bending strength and bending strain were measured according to ASTM D 638, and the type I energy release rate was measured according to ASTM D5045; the type I energy release rate of the toughened interface was measured according to ASTM D5528, the type II energy release rate was measured according to HB 7403, and the interlayer shear strength was measured according to ASTM D2344.
[0082] Table 1 Performance of Examples 1-2 and Comparative Examples 1-4
[0083]
[0084]
[0085] As shown in Table 1, compared with the comparative example, all the properties of the embodiment are improved. Due to the low dielectric properties of the added material itself and the interlayer toughening structure prepared using the method of the present invention has a unique pearl layer brick-slurry structure, therefore, the interlayer pearl layer bionic toughening structure of the present invention has low dielectric constant and low dielectric loss while also having good mechanical properties. In addition, the interfacial energy release rate and interlayer shear strength are significantly improved, indicating that the interlayer interface toughened by the interlayer phase of the present invention has excellent resistance to crack generation and expansion, significantly improves the interlayer fracture toughness of the composite material, and has broad application prospects.
[0086] In the present invention, the nacre bionic toughening structure between the layers of the high-speed impact-resistant wave-transmitting composite material can improve the overall modulus of the material, and has a gain effect on the transmission of stress, thereby improving the overall bearing capacity of the structure; when the overall structure is impacted, the cracks extend between the layers, and when reaching the aerogel wall, the aerogel wall composed of α-ZrP sheets slips, pulls out, and breaks. These methods can reduce and eliminate the stress concentration generated at the tip of the crack extension, consume a lot of energy, and deflect, differentiate, and terminate the cracks, hindering the extension of the main cracks between the layers, thereby inhibiting the delamination. Further, the modulus of the α-ZrP sheet is quite different from that of the resin matrix, and such a large modulus difference alternating arrangement can also play an effective crack-stopping effect. Further, the aerogel plays a role in expanding the interlayer space between the layers, so that the glue content between the composite layers increases, so that the cracks are more difficult to extend to the relatively fragile interface, so that the overall performance and anti-delamination performance of the material can be effectively improved. Further, the special orientation structure constructed by α-ZrP between the layers can show obvious interface effects. At the same time, α-ZrP, as a low dielectric material, is filled between the layers of the composite material in the form of aerogel, which can reduce the dielectric value of the interlayer phase.
[0087] The above is only a specific implementation of the present disclosure, which enables those skilled in the art to understand or implement the present disclosure. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.
Claims
1. A nacre bionic toughening structure between layers of a high-speed impact-resistant wave-transmitting composite material, characterized in that: It comprises an upper composite material (1), a lower composite material (3), and an interlayer nacre bionic toughening structure (2) constructed between the upper and lower composite material layers by a low dielectric sheet material and a resin matrix, which has the characteristics of preventing crack extension, improving interlayer performance, and having a low dielectric high-performance soft-hard alternating nacre structure similar to that of shells in nature; The upper composite material (1) is selected from one of a fiber-reinforced resin-based composite material, a foam material and a honeycomb material; The lower layer composite material (3) is selected from one of a fiber-reinforced resin-based composite material, a foam material and a honeycomb material; The interlayer nacre bionic toughening structure (2) is an aerogel completely filled with resin; the aerogel is an aerogel with directional orientation in a direction perpendicular to the horizontal direction, uniform wall thickness, and uniform pore distribution obtained by directional freezing of an aqueous dispersion system of α-ZrP nanosheets and cellulose after in-situ exfoliation; in the aqueous dispersion system of α-ZrP nanosheets and cellulose for preparing the aerogel, the mass ratio of α-ZrP to cellulose is 10~5:2~1; the interlayer nacre bionic toughening structure (2) is to assemble the α-ZrP sheets into a continuous network structure with a specific orientation direction by directional freezing technology, and further fill the resin matrix into the network structure, so that the resin matrix finally constitutes a soft layer and the oriented α-ZrP aerogel wall constitutes a hard layer, thereby constructing a soft-hard alternating nacre-like structure between the composite material layers; The soft layer can bond the aerogel into a whole and maintain a certain shape, transfer interlayer stress, and protect the aerogel from external erosion and damage; The low-dielectric oriented α-ZrP hard layer filled between the composite material layers in the form of aerogel has the function of improving the mechanical properties and wave transmission performance of the interlayer toughening structure. In addition, when the overall structure is impacted, the cracks are deflected, differentiated, and terminated, hindering the expansion of the main cracks between the layers, thereby effectively inhibiting delamination; The resin matrix is a thermosetting resin system obtained by uniformly mixing a thermosetting resin, a curing agent and a reaction aid; the thermosetting resin is selected from at least one of epoxy resin, unsaturated polyester resin and phenolic resin; the reaction aid includes any one or more mixtures of initiators, promoters and catalysts.
2. The nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 1, characterized in that: Cellulose acts as a structural reinforcement framework for oriented α-ZrP aerogels and can enhance the structure of oriented α-ZrP aerogels; The in-situ exfoliated α-ZrP nanosheets are exfoliated by using small molecule substances containing amino groups as exfoliants and utilizing ultrasound-assisted exfoliation technology to exfoliate the original α-ZrP nanosheets, and α-ZrP nanosheets of different two-dimensional sizes and thicknesses are finally obtained by controlling the exfoliation time and ultrasound power; The cellulose is selected from at least one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose and bacterial cellulose.
3. The nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 2, characterized in that: The stripping agent is selected from at least one of triethanolamine, ethylenediamine and lysine.
4. The nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 2, characterized in that: The α-ZrP nanosheet is a nanometer-level two-dimensional sheet material with a two-dimensional sheet size of 300-1700 nm and a sheet thickness of 30-100 nm. The α-ZrP aerogel has a thickness of 0.1-0.4 mm and a surface density of 20-100 g / m 2 .
5. The nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 1, characterized in that: The thickness of the interlayer nacre bionic toughening structure is 0.1-0.4 mm, the dielectric constant is 2.45-2.72, the loss tangent is 0.028-0.042, the bending strength is 100-130 MPa, the maximum bending strain is 4-6%, and the type I critical energy release rate is 1.02-1.58 kJ / m 2 ; The critical energy release rate of type I bonding interface is 0.7~1.2 kJ / m 2 The critical energy release rate of type II bonding interface is 3.0~3.8 kJ / m 2 , the interlaminar shear strength reaches 55~75 MPa.
6. The simplified preparation process of the nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to any one of claims 1 to 5, characterized in that: The steps include: (1) Dispersing α-ZrP powder uniformly in water, adding a certain amount of stripping agent, and stirring until the dispersion is uniform and free of precipitation to obtain an intercalated α-ZrP dispersion; transferring the dispersion to a cell disruptor, controlling the ultrasonic power and ultrasonic time, and obtaining α-ZrP dispersions with different stripping degrees; (2) adding cellulose to the stripped α-ZrP dispersion obtained in step (1) and completely dissolving the cellulose to obtain a uniform water dispersion system; pouring the obtained uniform water dispersion system into a copper bottom mold parallel to the ground so that the liquid nitrogen covers the copper bottom, and after the water dispersion system is completely frozen, transferring the mold to a freeze dryer, and removing the mold after drying to obtain an α-ZrP aerogel; (3) Mixing the thermosetting resin and the curing agent, mechanically stirring until the color is uniform and without stratification, then adding the reaction aid, mechanically stirring until the color is uniform; then vacuum degassing in an oven until no bubbles are generated to obtain a resin glue solution; (4) impregnating the α-ZrP aerogel prepared in step (2) into the resin glue prepared in step (3), evacuating the air so that the resin completely fills the aerogel, raising the temperature to perform pre-curing when there are no bubbles, and taking out the aerogel after the resin matrix is gelled to obtain a pre-cured body of the interlayer nacre bionic toughening structure; (5) placing the precured body of the interlayer nacre bionic toughening structure obtained in step (4) between the layers of two composite materials to be bonded, and using liquid molding or autoclave technology to solidify the interlayer toughening phase and the two composite materials as a whole, thereby obtaining a nacre bionic toughening structure between the layers of a high-speed impact-resistant and wave-transparent composite material.
7. The simplified preparation process of the nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 6, characterized in that: In step (1), the power of the cell disruptor is 150~300W, and the ultrasonic time is 3~15min; in step (2), the temperature of the liquid nitrogen is -196°C; the vacuum degree of the freeze-drying is -0.05~-0.09MPa, the temperature is -65~-45°C, and the time is 36~48h.
8. The simplified preparation process of the nacre bionic toughening structure between layers of the high-speed impact resistant and wave-transmitting composite material according to claim 6, characterized in that: In step (4), the vacuum degree of vacuum pumping is -0.09 MPa, the vacuum rate is 2 L / min, the temperature is 60 ~ 80 ° C, and the vacuum pumping time is 0.5 ~ 1 h.
Citation Information
Patent Citations
Substrate and preparation method thereof, light-emitting device, and display screen
CN109980127A
Metal ion / zirconium phosphate aerogel, preparation method thereof and composite phase change energy storage material
CN111841457A
Toughening material for prepreg, high-toughness composite material and preparation method thereof
CN112677602A
Preparation method of imitation pearl layer MXene / epoxy nano composite material
CN115286898A
Graphene-bacterial cellulose-MXene hybrid aerogel and preparation thereof, and epoxy resin-based composite material and preparation thereof