A super-tough flame-retardant polycarbonate composite material and preparation method thereof
By using silicone polymers as flame retardant-toughening additives in polycarbonate materials, combined with polybutylene terephthalate, the problems of easy cracking and insufficient fire resistance in polycarbonate material processing are solved, and efficient The flame retardant and toughening effects meet the environmental requirements of halogen-free, low toxicity and low smoke.
Patent Information
- Application Number
- CN202410323965.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Existing polycarbonate materials are prone to cracking during processing and have insufficient fire resistance, and traditional halogen-containing flame retardants are subject to environmental restrictions. It is necessary to develop non-toxic, environmentally friendly flame retardant and toughening additives to improve material performance.
Silicone polymer is used as a flame retardant-toughening additive. Its molecular backbone contains Si-O bonds and benzene ring-Si-benzene ring structure. Combined with polybutylene terephthalate, ultra-high-performance polymers are prepared through a specific synthesis method. Tough flame-retardant polycarbonate composite material, including 80-99 parts of polycarbonate and 1-20 parts of flame-retardant-toughening additives, is processed at high temperature to improve material performance.
It achieves good flame retardant properties, high temperature oxidation resistance and excellent mechanical properties of the material, while meeting the requirements of halogen-free, low toxicity and low smoke, improving the overall performance of polycarbonate materials and meeting green environmental protection standards.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and particularly relates to an ultra-tough flame-retardant polycarbonate composite material and a preparation method thereof. Background Art
[0002] Polycarbonate (PC) is a kind of thermoplastic engineering plastic. Its molecular chain contains both a relatively rigid benzene ring structure and a relatively flexible ether bond. This special molecular chain structure makes polycarbonate have high strength and heat resistance, as well as high toughness. PC is an amorphous polymer with high transparency, good gloss, excellent dimensional stability, and low molding shrinkage. Without any modification, PC itself can reach the UL94 V-2 flame retardant rating. Because of these excellent properties, PC is widely used in optical lighting, home appliance housings, power tool housings, electronic appliances, automotive interiors, bumpers, etc. However, PC has poor processing fluidity, and the internal stress is not easy to release during molding, which easily leads to stress concentration and cracking of the product.
[0003] In order to improve the fire resistance and mechanical properties of PC, adding additives such as flame retardants and toughening agents is a relatively simple method. In the past, halogen-containing compounds were often used for flame retardant modification of PC, and were very effective for PC flame retardancy, but due to environmental issues and other reasons, halogen-containing flame retardants were restricted in use. As a substitute for halogen-containing flame retardants, phosphorus-containing, sulfur-containing and silicon-containing flame retardants have now been developed. Among them, silicon-based flame retardants can be roughly divided into four categories: modified SiO2, polysilane, polysiloxane, and silsesquioxane. As a rising star in the flame retardant family, this type of flame retardant has the characteristics of high efficiency, non-toxicity, anti-drip, smoke suppression, etc., and can effectively improve material processing and heat resistance, and can also effectively improve the mechanical properties of polycarbonate materials. With the enhancement of people's environmental awareness and the improvement of the relevant legal system, it is quite urgent to develop non-toxic and environmentally friendly additives with both flame retardant and toughening effects to improve the performance of polycarbonate materials. Therefore, it is necessary to develop a new type of ultra-tough temperature flame retardant polycarbonate composite material. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an ultra-tough flame-retardant polycarbonate composite material and a preparation method thereof.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] In one aspect, the present application provides an ultra-tough flame-retardant polycarbonate composite material, the ultra-tough flame-retardant polycarbonate composite material comprising polycarbonate and a flame retardant-toughening additive;
[0007] The flame retardant-toughening additive comprises an organic silicon polymer, and the main molecular chain of the organic silicon polymer comprises both an inorganic structure of Si-O bonds and an organic structure of benzene ring-Si-benzene ring.
[0008] Further, the ultra-tough flame-retardant polycarbonate composite material comprises, by weight, 80-99 parts of the polycarbonate and 1-20 parts of the flame-retardant-toughening additive;
[0009] Preferably, the ultra-tough flame-retardant polycarbonate composite material comprises, by weight, 90-99 parts of the polycarbonate and 1-10 parts of the flame-retardant-toughening additive;
[0010] Further, the organosilicon polymer is obtained by polymerizing di(4-(dimethylhydroxysilyl)phenyl)dimethylsilane and diphenyldimethoxysilane;
[0011] Furthermore, the ultra-tough flame-retardant polycarbonate composite material also includes polybutylene terephthalate;
[0012] Preferably, the ultra-tough flame-retardant polycarbonate composite material comprises, by weight, 80-98 parts of the polycarbonate, 1-10 parts of the polybutylene terephthalate and 1-10 parts of the flame retardant-toughening additive;
[0013] Furthermore, the preparation method of the organosilicon polymer comprises the following steps:
[0014] Step S3: mixing solvent A, diphenyldimethoxysilane, di(4-(dimethylethoxysilyl)phenyl)dimethylsilane, water and an acid catalyst to react, and after the reaction is completed, purifying to obtain the organosilicon polymer;
[0015] Further, the mass ratio of the di(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the diphenyldimethoxysilane is 0.5-1.5:1;
[0016] Preferably, the mass ratio of the di(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the diphenyldimethoxysilane is 1:1;
[0017] Further, the mass ratio of the bis(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the water is 5-15:1;
[0018] Further, the mass ratio of the bis(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the acid catalyst is 15-30:1;
[0019] Further, the solvent A includes one or more of toluene, isopropanol, ethanol, THF, 1,2-dichloroethane, and ethylene glycol;
[0020] Further, the acid catalyst includes one or more of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid;
[0021] Furthermore, the reaction time of step S3 is 2-4h, and the reaction temperature is 20-30°C;
[0022] Furthermore, the method for preparing the organosilicon polymer further comprises the following steps:
[0023] Step S2: adding a small amount of di(4-bromophenyl)dimethylsilane to solvent B, and then adding magnesium chips and iodine particles, reacting at 35-45° C. for 0.3-0.7 h, and then adding to a mixed solution of dimethylethoxychlorosilane and the remaining amount of di(4-bromophenyl)dimethylsilane, and after the reaction is completed, obtaining di(4-(dimethylethoxysilyl)phenyl)dimethylsilane;
[0024] Further, in step S2, the remaining amount of di(4-bromophenyl)dimethylsilane accounts for 85%-95% of the total amount of di(4-bromophenyl)dimethylsilane added, and the small amount of di(4-bromophenyl)dimethylsilane accounts for 5%-15% of the total amount of di(4-bromophenyl)dimethylsilane added;
[0025] Further, the total molar ratio of the dimethylethoxychlorosilane to the bis(4-bromophenyl)dimethylsilane is 2-2.2:1;
[0026] Further, the solvent B includes one or more of toluene, isopropanol, ethanol, THF, 1,2-dichloroethane, and ethylene glycol;
[0027] Furthermore, the step S2 is carried out under reflux conditions, and the reaction time is 3-5h;
[0028] Furthermore, the method for preparing the organosilicon polymer further comprises the following steps:
[0029] Step S1: taking dimethyldichlorosilane, and then adding ethanol to react, and after the reaction is completed, obtaining dimethylethoxychlorosilane; wherein the molar ratio of the dimethyldichlorosilane to the ethanol is 0.9-1.1:1;
[0030] Furthermore, the step S1 is carried out at 20-30°C for 1-3h;
[0031] On the other hand, the present application also provides a method for preparing an ultra-tough flame-retardant polycarbonate composite material, comprising the following steps: taking raw materials, mixing them evenly, and subjecting them to high-temperature treatment, and obtaining a polycarbonate composite material after the treatment is completed;
[0032] The raw materials include polycarbonate and a flame retardant-toughening additive; the flame retardant-toughening additive includes an organic silicon polymer, and the main molecular chain of the organic silicon polymer includes both an inorganic structure of Si-O bonds and an organic structure of benzene ring-Si-benzene ring;
[0033] Further, the raw materials, by weight, include 80-99 parts of the polycarbonate and 1-20 parts of the flame retardant-toughening additive;
[0034] Furthermore, the raw materials also include polybutylene terephthalate;
[0035] Preferably, the ultra-tough flame-retardant polycarbonate composite material comprises, by weight, 80-99 parts of the polycarbonate, 1-10 parts of the polybutylene terephthalate and 1-10 parts of the flame retardant-toughening additive;
[0036] Furthermore, the raw materials are placed in a vacuum oven at 120° C. for vacuum drying for 20-28 hours, and then the raw materials are mixed evenly;
[0037] Furthermore, the conditions of the high temperature treatment are: stirring treatment at a temperature of 240-260° C. for 6-10 minutes.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] The invention discloses an ultra-tough flame-retardant polycarbonate composite material and a preparation method thereof. The polycarbonate composite material comprises polycarbonate and a flame-retardant-toughening additive, wherein the flame-retardant-toughening additive comprises an organosilicon polymer, the molecular main chain of the organosilicon polymer comprises both an inorganic structure of a Si-O bond and an organic structure of a benzene ring-Si-benzene ring, and has the dual properties of an inorganic compound and an organic polymer. As an additive, the organosilicon polymer can not only impart good flame-retardant properties, high-temperature oxidation resistance and excellent mechanical properties to a substrate, but is also eco-friendly and does not release toxic and harmful gases into the environment during combustion, thus meeting the flame-retardant requirements of halogen-free, low-toxicity and low-smoke as well as the current requirements of green environmental protection. DETAILED DESCRIPTION
[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present invention, and the terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. In the description of the present application, it should be understood that "and / or" describes the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In the present application, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, c can be single or multiple, respectively.
[0042] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and cannot be used as a limitation of the present application.
[0043] Example 1
[0044] This embodiment provides a novel flame retardant-toughening additive, which is prepared by the following steps:
[0045] Step S1, preparation of dimethylethoxychlorosilane:
[0046] Take 4 mol of dimethyldichlorosilane, add 4 mol of anhydrous ethanol dropwise at room temperature (25°C) under nitrogen protection, add the solution over 2 h, continue stirring for 2 h, and distill to obtain dimethylethoxychlorosilane;
[0047] Step S2, preparation of bis(4-(dimethylethoxysilyl)phenyl)dimethylsilane:
[0048] First, add 2.2 mol of dimethylethoxychlorosilane and 0.9 mol of di(4-bromophenyl)dimethylsilane to THF, mix well and set aside; then add 0.1 mol of di(4-bromophenyl)dimethylsilane to THF, add 2.2 mol of magnesium chips and several grains of iodine under nitrogen protection, stir and react at 40°C for 0.5h, then slowly add dropwise to the above mixed solution, keep the reaction temperature at about 80°C, add dropwise for about 3h, then reflux for 6h, after the reaction is completed, purify to obtain di(4-(dimethylethoxysilyl)phenyl)dimethylsilane;
[0049] Step S3, preparation of novel flame retardant-toughening additive:
[0050] 50 parts by weight of toluene, 10 parts by weight of diphenyldimethoxysilane, 10 parts by weight of di(4-(dimethylethoxysilyl)phenyl)dimethylsilane, 1 part by weight of deionized water and 0.4 parts by weight of concentrated sulfuric acid catalyst are mixed evenly, and then mechanically stirred for reaction at room temperature for 3 hours. After the reaction is completed, the mixture is washed with water and then the solvent toluene is removed by reduced pressure distillation to obtain an organosilicon polymer, i.e., a new flame retardant-toughening additive.
[0051] Application Examples 1-5
[0052] Application Example 1-5 provides an ultra-tough flame-retardant polycarbonate composite material, which is prepared by the following steps:
[0053] PC (polycarbonate), PBT (polybutylene terephthalate) and a novel flame retardant-toughening additive were placed in a vacuum oven at 120°C and vacuum dried for 24 hours. Then, PC, PBT and the novel flame retardant-toughening additive were weighed and mixed evenly according to the formula in Table 1 below. The mixed raw materials were added to an internal mixer for melt blending. The internal mixing temperature was 250°C, the speed was 80r / min, and the time was 8min to obtain an ultra-tough flame retardant polycarbonate composite material. The obtained polycarbonate composite material was then pressed into a sheet using a plate press and cut into strips for vertical burning, LOI test, thermogravimetric (TG) analysis, tensile property test, and notched impact strength test.
[0054] Table 1
[0055] PC (parts by weight) PBT (parts by weight) Flame retardant-toughening additives (parts by weight) Application Example 1 95 0 5 Application Example 2 90 0 10 Application Example 3 85 5 10 Application Example 4 85 10 5 Application Example 5 80 10 10
[0056] Comparative Example 1
[0057] Compared with Application Example 1, the only difference is that the organosilicon polymer prepared in Example 1 is not added.
[0058] Performance Testing
[0059] Vertical combustion was tested according to GB / T 2048-2008, and the results are shown in Table 2;
[0060] The limiting oxygen index test (LOI) was tested according to ASTM D2863 standard, and the results are shown in Table 2;
[0061] Thermogravimetric analysis (TG): carried out under nitrogen atmosphere, with a gas flow rate of 20 mL / min, a temperature range of 30-800 °C, and a heating rate of 10 °C / min. The results are shown in Table 2;
[0062] The tensile properties were tested according to GB / T 1040.1-2018, and the tensile setting was 50 mm / min. The results are shown in Table 2;
[0063] The notched impact strength was tested according to GB / T 1843-2008, the specimen size was 100 mm × 10 mm × 4 mm, the notch was A-type notch, and the notch retention width was 8 mm. The results are shown in Table 2;
[0064] Table 2
[0065]
[0066] As can be seen from Table 2, the vertical combustion rating, LOI value, tensile strength, elongation at break and notched impact strength of the polycarbonate composite materials prepared in Application Examples 1-5 of the present invention are better than those of Comparative Example 1. In addition, when the polycarbonate composite materials prepared in Application Examples 1-5 of the present invention lose 5% of their weight, the corresponding temperatures are also significantly higher than those of Comparative Example 1. It can be seen that the high temperature resistance, flame retardancy and toughness of the polycarbonate composite materials obtained by compounding the flame retardant-toughening additive prepared in the present application with PC and the like are significantly improved.
[0067] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application, and the scope of protection of the present invention shall be based on the scope defined by the claims. For those of ordinary skill in the art, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the scope of protection of the present invention. Those of ordinary skill in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. An ultra-tough flame-retardant polycarbonate composite material, It is characterized in that The ultra-tough flame-retardant polycarbonate composite material comprises polycarbonate, a flame-retardant-toughening additive and polybutylene terephthalate; The flame retardant-toughening additive comprises an organic silicon polymer, and the preparation method of the organic silicon polymer comprises the following steps: step S3: mixing solvent A, diphenyldimethoxysilane, di(4-(dimethylethoxysilyl)phenyl)dimethylsilane, water and an acid catalyst for reaction, and purifying after the reaction to obtain the organic silicon polymer; the mass ratio of the di(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the diphenyldimethoxysilane is 0.5-1.5:1; the di(4 The mass ratio of bis(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the water is 5-15:1; the mass ratio of bis(4-(dimethylhydroxysilyl)phenyl)dimethylsilane to the acid catalyst is 15-30:1; the solvent A comprises one or more of toluene, isopropanol, ethanol, THF, 1,2-dichloroethane, and ethylene glycol; the acid catalyst comprises one or more of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid; the reaction time of step S3 is 2-4h, and the reaction temperature is 20-30°C; The ultra-tough flame-retardant polycarbonate composite material comprises, by weight, 80-98 parts of the polycarbonate, 1-10 parts of the polybutylene terephthalate and 1-10 parts of the flame-retardant-toughening additive.
2. The ultra-tough flame-retardant polycarbonate composite material according to claim 1, It is characterized in that The method for preparing the organosilicon polymer further comprises the following steps: Step S2: Add a small amount of di(4-bromophenyl)dimethylsilane to solvent B, then add magnesium chips and iodine particles, react at 35-45°C for 0.3-0.7h, then add to a mixed solution of dimethylethoxychlorosilane and the remaining amount of di(4-bromophenyl)dimethylsilane to react, and after the reaction is completed, di(4-(dimethylethoxysilyl)phenyl)dimethylsilane is obtained.
3. The ultra-tough flame-retardant polycarbonate composite material according to claim 2, It is characterized in that In the step S2, the remaining amount of di(4-bromophenyl)dimethylsilane accounts for 85%-95% of the total amount of di(4-bromophenyl)dimethylsilane added, and the small amount of di(4-bromophenyl)dimethylsilane accounts for 5%-15% of the total amount of di(4-bromophenyl)dimethylsilane added; And / or, the total molar ratio of the dimethylethoxysilyl chloride to the bis(4-bromophenyl)dimethylsilane is 2-2.2:
1.
4. The ultra-tough flame-retardant polycarbonate composite material according to claim 2, It is characterized in that In the step S2, the solvent B includes one or more of toluene, isopropanol, ethanol, THF, 1,2-dichloroethane, and ethylene glycol; And / or, the step S2 is carried out under reflux conditions for a reaction time of 3-5 hours.
5. The ultra-tough flame-retardant polycarbonate composite material according to any one of claims 2 to 4, It is characterized in that The method for preparing the organosilicon polymer further comprises the following steps: Step S1: Take dimethyldichlorosilane, then add ethanol to react, and after the reaction is completed, dimethylethoxychlorosilane is obtained.
6. The ultra-tough flame-retardant polycarbonate composite material according to claim 5, It is characterized in that The molar ratio of the dimethyldichlorosilane to the ethanol is 0.9-1.1; And / or, the step S1 is carried out at 20-30° C. for 1-3 h.