A high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy and its preparation method
By heating and melting electrolytic copper, copper-chromium alloy, and copper-zirconium alloy under a reducing atmosphere, and controlling the alloy melt temperature and feeding sequence, a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy was prepared. This solved the problems of low zirconium yield and severe oxidation loss, and achieved the preparation of alloys with high strength and high conductivity.
Patent Information
- Application Number
- CN202410583800.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-05-11
AI Technical Summary
In the existing technology, the yield of zirconium in copper-chromium-zirconium alloy is low and the oxidation loss is serious during the preparation process, making it difficult to use in large-size ingots. Furthermore, vacuum melting is not conducive to industrial promotion, while non-vacuum melting is difficult to effectively control the oxidation reaction.
Electrolytic copper, copper-chromium alloy, copper-zirconium alloy, and copper-magnesium alloy are used as raw materials. They are heated and melted in a reducing atmosphere. The temperature of the alloy melt and the order of feeding are controlled. The distribution of zirconium and its electrical conductivity are improved by adding copper-magnesium alloy. Combined with the post-processing steps of the alloy, the oxygen content is reduced.
This significantly improves the electrical conductivity and strength of copper-chromium-zirconium alloys, reduces oxygen content and zirconium oxidation loss, and enables the preparation of high-strength and high-conductivity copper-chromium-zirconium-magnesium alloys.
Smart Images

Figure CN118222864B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical technology, specifically relating to a high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy and its preparation method. Background Technology
[0002] Currently, the preparation of copper-chromium-zirconium alloys both domestically and internationally mainly employs two methods: vacuum melting and non-vacuum melting. While the vacuum melting environment effectively isolates Zr from O2, ensuring Zr yield, it hinders industrial-scale promotion, mass production, and cost control, and also prevents the production of large-sized ingots for rolling. Non-vacuum melting, on the other hand, makes it difficult to control the isolation between Zr and O2, as Zr easily absorbs O2 during heating, leading to severe Zr burn-off. Existing technologies address the problem caused by Zr contacting O2 by introducing inert gases such as argon into the melting furnace to create a protective atmosphere, thereby reducing oxidation reactions and burn-off of Cr and Zr elements, particularly Zr burn-off. However, due to the furnace material itself, oxide inclusions in copper and alloy feedstock, and air introduced during charging, Zr can still react with O, resulting in severe burn-off and difficulty in effectively reducing the oxygen content in the melt. Therefore, developing a product that solves these technical problems is essential. Summary of the Invention
[0003] The first objective of this invention is to provide a high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy; the second objective is to provide a method for preparing the aforementioned high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy.
[0004] The first objective of this invention is achieved as follows: the high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy is prepared by using electrolytic copper, copper-chromium alloy, copper-zirconium alloy and copper-magnesium alloy as raw materials, through alloying and post-treatment steps. The copper-chromium alloy contains 8-12% chromium, the copper-zirconium alloy contains 30-50% zirconium, and the copper-magnesium alloy contains 10-30% magnesium.
[0005] The second objective of this invention is achieved by including alloying and post-processing steps, specifically including: A. Alloy: The raw material electrolytic copper according to the formula is placed in a medium-frequency induction furnace and heated to complete melting of copper under a reducing atmosphere to obtain material a, with the temperature controlled at 1150±15℃; the raw material copper-chromium alloy according to the formula is added and heated to melt of copper-chromium alloy to obtain material b, with the temperature controlled at 1200±15℃; then the raw material copper-magnesium alloy according to the formula is added and heated to melt of copper-magnesium alloy to obtain material c, with the temperature controlled at 1200±15℃; finally, the raw material copper-zirconium alloy according to the formula is added, stirred and held at the temperature for 3~5 minutes to obtain high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d; B. Post-processing: The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested before being poured into the furnace.
[0006] The beneficial effects of this invention are as follows: 1. This invention uses electrolytic copper, copper-chromium alloy, copper-zirconium alloy, and copper-magnesium alloy materials to heat and melt under reducing conditions. By comprehensively controlling the alloy melt temperature, the order and proportion of adding copper-chromium alloy, copper-zirconium alloy, and copper-magnesium alloy, as well as the adding tools and furnace feeding methods, it effectively overcomes the disadvantages of chromium being difficult to dissolve and zirconium having a high melting point and absorbing a large amount of oxygen during heating, resulting in low zirconium yield. This invention significantly reduces the oxygen content and oxidation loss of zirconium in copper-chromium-zirconium alloys.
[0007] 2. This invention supplements Cr and Zr elements by using intermediate alloys such as copper-chromium alloys and copper-zirconium alloys. Compared with pure metals such as zirconium particles, this not only reduces the alloy melting temperature and reduces oxidation caused by exposure to air before and during feeding, but also increases the dispersion rate of Cr and Zr elements in the alloy. This ensures that the chromium and zirconium in the obtained alloy are more uniformly distributed, thereby significantly improving the electrical conductivity and strength of the copper-chromium-zirconium alloy.
[0008] 3. By incorporating a copper-magnesium alloy, this invention, compared to the Cu-Cr alloy, resulted in a recovery phase during the aging process of the 60% cold-deformed Cu-Cr-Mg alloy at most temperatures. This is because the Cu-Cr-Mg alloy has a higher dislocation density after rolling with the same deformation, increasing the driving force for recovery. Furthermore, the Mg element delays the recrystallization process, extending the duration of the recovery process and resulting in a more pronounced recovery. During the mid- and late-stage aging, the hardness change of the Cu-Cr-Mg alloy is relatively gradual, exhibiting a prolonged hardness plateau. This is because the Mg element hinders the precipitation and growth of precipitates, resulting in finer, more dispersed, and denser precipitates that, together with Mg atoms, effectively pinnate dislocation movement and interface migration, stabilizing the deformed microstructure of the alloy. The conductivity change during aging is similar to that of the Cu-Cr binary alloy. The addition of Mg element influences the limiting conductivity of the alloy to some extent, typically around 80% IACS.
[0009] Since Mg is insoluble in Cr and does not react to form a new phase, Mg atoms in the Cr-rich precipitate will be gradually expelled from the precipitate during aging. Mg has no solid solubility in Cr but over 2% in Cu, therefore the diffusion coefficient of Mg in Cr is much greater than that in Cu. Within a short time, Mg atoms will be expelled from the precipitate. During this period, Mg cannot diffuse into the copper matrix and thus accumulates at the precipitate-matrix interface, leading to Mg segregation on the precipitate surface. This segregated Mg will fill the vacancies between the precipitate and the matrix, effectively reducing mismatch, alleviating interfacial elastic distortion, reducing the phase transformation driving force, stabilizing the intermediate phase, and delaying the phase transformation process in the later stages of aging. Attached Figure Description
[0010] Figure 1 This is a schematic diagram of the process flow of the present invention; Figure 2 This is a schematic diagram of the metallographic structure of the copper-chromium-zirconium-magnesium alloy of the present invention. Detailed Implementation
[0011] The present invention will be further described below with reference to embodiments, but in no way shall the present invention be limited. The examples described herein are merely descriptions of preferred experimental methods of the present invention and are not intended to limit the concept and scope of the present invention. Any modifications and improvements made based on the teachings of the present invention without departing from the design concept of the present invention shall fall within the scope of the present invention.
[0012] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy of the present invention is prepared by using electrolytic copper, copper-chromium alloy, copper-zirconium alloy and copper-magnesium alloy as raw materials, through alloying and post-treatment steps. The copper-chromium alloy has a chromium content of 8-12%, the copper-zirconium alloy has a zirconium content of 30-50%, and the copper-magnesium alloy has a magnesium content of 10-30%.
[0013] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy has the following composition: 0.1-1% chromium, 0.02-0.2% zirconium, 0.1-0.4% magnesium, with the remainder being copper and unavoidable impurities.
[0014] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy has a strength of 630 MPa or higher and a conductivity of 75% IACS or higher.
[0015] The preparation method of the high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy of the present invention includes alloying and post-processing steps, specifically including: A. Alloy: The raw material electrolytic copper according to the formula is placed in a medium-frequency induction furnace and heated to complete melting of copper under a reducing atmosphere to obtain material a, with the temperature controlled at 1150±15℃; the raw material copper-chromium alloy according to the formula is added and heated to melt of copper-chromium alloy to obtain material b, with the temperature controlled at 1200±15℃; then the raw material copper-magnesium alloy according to the formula is added and heated to melt of copper-magnesium alloy to obtain material c, with the temperature controlled at 1200±15℃; finally, the raw material copper-zirconium alloy according to the formula is added, stirred and held at the temperature for 3~5 minutes to obtain high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d; B. Post-processing: The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested before being poured into the furnace.
[0016] The reducing atmosphere is achieved by placing 10-20 mm of carbon powder on the surface of the electrolytic copper.
[0017] The sampling and testing method involves using a sampling spoon to extract samples from the high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy melt for composition analysis.
[0018] The casting temperature is 1200±10℃.
[0019] The present invention will be further described below with reference to specific embodiments: Comparative Example 1 According to the mass fraction of chromium and zirconium (0.5% chromium, 0.1% zirconium), the raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 8.2%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then a copper-zirconium alloy (zirconium content of 30.4%) is added, stirred and kept at a temperature of 3-5 min to obtain high-strength and high-conductivity copper-chromium-zirconium alloy melt d. The copper-chromium-zirconium alloy melt d is sampled and tested (alloy composition: chromium: 0.43%, zirconium 0.08%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium alloy.
[0020] The high-strength, high-conductivity copper-chromium-zirconium alloy prepared in this embodiment has a strength of 480 MPa and a conductivity of 63% IACS.
[0021] Example 1 The raw materials are prepared according to the mass fraction of chromium and zirconium (0.5% chromium, 0.1% zirconium, and 0.1% magnesium). The raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 10.4%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then a magnesium alloy is added, and the temperature is raised until the copper-magnesium alloy (magnesium content of 10.5%) melts to obtain material c, and the temperature is controlled at 1200±15℃. Finally, a copper-zirconium alloy (zirconium content of 35.6%) is added, stirred, and kept at a temperature of 3-5 min to obtain a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d. The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested (alloy composition: chromium: 0.35%, zirconium: 0.08%, magnesium: 0.09%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium alloy.
[0022] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy prepared in this embodiment has a strength of 675 MPa and a conductivity of 75% IACS.
[0023] Example 2 The raw materials are prepared according to the mass fraction of chromium and zirconium (0.5% chromium, 0.1% zirconium, and 0.2% magnesium). The raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 10.4%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then, a magnesium alloy is added, and the temperature is raised until the copper-magnesium alloy (magnesium content of 10.5%) melts to obtain material c, and the temperature is controlled at 1200±15℃. Finally, a copper-zirconium alloy (zirconium content of 35.6%) is added, stirred, and kept at a temperature of 3-5 min to obtain a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d. The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested (alloy composition: chromium: 0.35%, zirconium: 0.08%, magnesium: 0.15%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy.
[0024] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy prepared in this embodiment has a strength of 653 MPa and a conductivity of 80% IACS.
[0025] Example 3 The raw materials are prepared according to the mass fraction of chromium and zirconium (0.5% chromium, 0.1% zirconium, and 0.4% magnesium). The raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 10.4%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then, a magnesium alloy is added, and the temperature is raised until the copper-magnesium alloy (magnesium content of 10.5%) melts to obtain material c, and the temperature is controlled at 1200±15℃. Then, a copper-zirconium alloy (zirconium content of 35.6%) is added, stirred, and kept at a temperature of 3-5 min to obtain a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d. The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested (alloy composition: chromium: 0.35%, zirconium: 0.08%, magnesium: 0.36%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy.
[0026] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy prepared in this embodiment has a strength of 683 MPa and a conductivity of 82% IACS.
[0027] Example 4 According to the mass fraction of chromium and zirconium (1% chromium, 0.1% zirconium, and 0.4% magnesium), the raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 10.4%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then, a magnesium alloy is added, and the temperature is raised until the copper-magnesium alloy (magnesium content of 10.5%) melts to obtain material c, and the temperature is controlled at 1200±15℃. Then, a copper-zirconium alloy (zirconium content of 35.6%) is added, stirred, and kept at a temperature of 3-5 minutes to obtain a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d. The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested (alloy composition: chromium: 0.84%, zirconium: 0.08%, magnesium: 0.37%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy.
[0028] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy prepared in this embodiment has a strength of 703 MPa and a conductivity of 83% IACS.
[0029] Example 5 According to the mass fraction of chromium and zirconium (1% chromium, 0.2% zirconium, and 0.4% magnesium), the raw material electrolytic copper is placed in a medium-frequency induction furnace, and 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. A copper-chromium alloy (chromium mass percentage of 10.4%) is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then, a magnesium alloy is added, and the temperature is raised until the copper-magnesium alloy (magnesium content of 10.5%) melts to obtain material c, and the temperature is controlled at 1200±15℃. Then, a copper-zirconium alloy (zirconium content of 35.6%) is added, stirred, and kept at a temperature of 3-5 minutes to obtain a high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy melt d. The copper-chromium-zirconium-magnesium alloy melt d is sampled and tested (alloy composition: chromium: 0.88%, zirconium: 0.17%, magnesium: 0.36%), and then poured out of the furnace to obtain the target high-strength and high-conductivity copper-chromium-zirconium-magnesium alloy.
[0030] The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy prepared in this embodiment has a strength of 685 MPa and a conductivity of 84% IACS.
Claims
1. A high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy, characterized in that, The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy is prepared by alloying and post-processing steps using electrolytic copper, copper-chromium alloy with 8-12% chromium content, copper-magnesium alloy with 10-30% magnesium content, and copper-zirconium alloy with 30-50% zirconium content as raw materials. The composition of the high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy is: 0.1-1% chromium, 0.1-0.4% magnesium, 0.02-0.2% zirconium, with the remainder being copper and unavoidable impurities. The alloying process is as follows: Electrolytic copper of the specified formula is placed in a medium-frequency induction furnace. 10-20 mm of carbon powder is placed on the surface of the electrolytic copper. The temperature is raised until the copper is completely melted to obtain material a, and the temperature is controlled at 1150±15℃. Copper-chromium alloy of the specified formula is added, and the temperature is raised until the copper-chromium alloy melts to obtain material b, and the temperature is controlled at 1200±15℃. Then, copper-magnesium alloy of the specified formula is added, and the temperature is raised until the copper-magnesium alloy melts to obtain material c, and the temperature is controlled at 1200±15℃. Finally, copper-zirconium alloy of the specified formula is added, stirred, and kept at this temperature for 3-5 minutes to obtain copper-chromium-zirconium-magnesium alloy melt d. The post-processing step is as follows: the copper-chromium-zirconium-magnesium alloy melt d is sampled and tested before being poured into the furnace. The cast high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy has a strength of over 630 MPa and a conductivity of over 75% IACS.
2. The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy according to claim 1, characterized in that, The sampling and testing method involves using a sampling spoon to extract samples from the high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy melt for composition analysis.
3. The high-strength, high-conductivity copper-chromium-zirconium-magnesium alloy according to claim 1, characterized in that, The casting temperature is 1200±10℃.
Citation Information
Patent Citations
Preparation method for Cu-Cr-Zr-Mg alloy bar
CN105714133A