A kind of ultra-high impact toughness hot-rolled medium manganese steel and heat treatment method thereof
The refined bainite and ferrite layered structures are formed through two-phase zone annealing heat treatment, which solves the problems of insufficient thermal stability and impact toughness caused by austenitization in the heat treatment of medium manganese steel, and significantly improves the quality of medium manganese steel. impact toughness and strength.
Patent Information
- Application Number
- CN202410513122.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-26
AI Technical Summary
During the traditional heat treatment process of medium manganese steel, austenitization results in insufficient thermal stability of the workpiece, and the impact toughness needs to be improved.
A two-phase zone annealing heat treatment method is adopted, including heating to 920°C, water quenching, annealing to 680~750°C, holding to 195~225°C and air cooling to form refined bainite, ferrite and retained austenite layers -like structure to improve the supercooling and stability of austenite.
Significantly improves the impact toughness and strength of medium manganese steel, delays fracture, and enhances mechanical properties. The tensile strength is 1090~1500MPa, the elongation is 22.8~46.5%, and the 20℃ V-notch impact absorption energy is 105~170J.
Smart Images

Figure CN118222943B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material processing, in particular to an ultra-high impact toughness hot-rolled medium manganese steel and a heat treatment method thereof. Background Art
[0002] Medium manganese steel is a new type of steel material that has emerged in recent years. It is considered to be the third generation of automotive steel due to its excellent mechanical properties. Medium manganese steel needs to be heat treated during processing. In traditional processes, the heat treatment process for medium manganese steel will use complete austenitization.
[0003] Austenitization is to heat the workpiece to a temperature above the eutectoid temperature, so that the ferrite and cementite at room temperature are transformed back to austenite. Austenite is an interstitial solid solution of carbon dissolved in γ-Fe. It has a large carbon solubility and regenerates steel into a uniform austenite structure. Austenite is a structure that can only exist stably at a high temperature greater than 727°C. It has good plasticity and is the structure required for most steel types when pressure processing is performed at high temperatures. However, the heat treatment of complete austenitization will make the thermal stability of the workpiece insufficient, and the impact toughness of the processed medium manganese steel needs to be strengthened. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an ultra-high impact toughness hot-rolled medium manganese steel and a heat treatment method thereof, so as to solve the problems raised in the above-mentioned background technology. The present invention enhances the thermal stability of austenite, increases the supercooling of austenite, enhances the nucleation driving force of bainite, and improves the impact toughness of steel.
[0005] In order to achieve the above-mentioned purpose, the present invention is realized through the following technical scheme: a kind of ultra-high impact toughness hot-rolled medium manganese steel, which contains the following components and their proportions: C: 0.04~0.43wt.%, Si: 0.36~1.40wt.%, Mn: 3.80~5.93wt.%, Al: 0.86~3.53wt.%, Nb: 0.04~0.08wt.%, Cr: 0.90~1.36wt.%, Ni: 0.85~1.65%, V: 0.11~0.19 wt.%, P≤0.010%, S≤0.002%, 0.17 wt.%≤Nb+ V≤0.25wt.%.
[0006] Furthermore, the medium manganese steel contains the following components and their proportions: C: 0.042wt.%, Si: 0.9wt.%, Mn: 4.80wt.%, Al: 2.5wt.%, Nb: 0.06wt.%, Cr: 1.1wt.%, Ni: 1.2%, V: 0.15 wt.%, P: 0.008%, S: 0.002%, Nb+V: 0.22 wt.%.
[0007] Furthermore, the medium manganese steel contains the following components and their proportions: C: 0.04wt.%, Si: 0.6wt.%, Mn: 4.2wt.%, Al: 1.2wt.%, Nb: 0.05wt.%, Cr: 1.2wt.%, Ni: 1.1%, V: 0.11 wt.%, P: 0.009%, S: 0.00018%, Nb+ V: 0.18 wt.%.
[0008] Furthermore, the metallographic structure of the medium manganese steel includes: bainite + martensite: 46.5~58.8 vol.%, ferrite: 17.3~23.5 vol.%, and retained austenite 23.4~30.3 vol.%.
[0009] A heat treatment method for preparing the above-mentioned medium manganese steel, the heat treatment method uses two-phase zone annealing, and specifically comprises the following steps: step 1, heating the processed medium manganese steel raw material to 920°C, keeping it warm at this temperature, and then water quenching it to room temperature; step 2, controlling the temperature to cool it to 680~750°C, and annealing it at this temperature; step 3, continuing to control the temperature to cool it to 195~225°C and keeping it warm under this temperature adjustment; step 4, air cooling it to room temperature.
[0010] Furthermore, the insulation time in step 1 is 15 minutes.
[0011] Furthermore, the annealing time in step 2 is 10 minutes.
[0012] Furthermore, the insulation time in step three is 12 to 24 hours.
[0013] Beneficial effects of the present invention:
[0014] 1. The refined bainite of the present invention forms a layered structure with ferrite and residual austenite. When impacted, the layered structure changes the crack propagation direction or passivates the crack, consumes a large amount of energy, causes delayed fracture of the sample, and improves its impact toughness performance.
[0015] 2. The stability of the retained austenite formed by the present invention is also greatly improved. The TRIP effect of the stable retained austenite during the impact process also consumes a lot of energy, improving the impact toughness of the steel. In addition, since the present invention contains 46.5-58.8 vol.%, and refines its structure, it also ensures that the strength of the steel is 1090-1500 MPa.
[0016] 3. The mechanical properties of the medium manganese steel prepared by the present invention are as follows: tensile strength: 1090~1500MPa; elongation: 22.8~46.5%, elongation: 18.8~30.5%, and 20°C V-notch impact absorption energy is 105~170J. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a flow chart of a heat treatment method for hot-rolled medium manganese steel with ultra-high impact toughness according to the present invention;
[0018] Figure 2 Figure 1 is a TEM image of the microstructure in an embodiment of the present invention. DETAILED DESCRIPTION
[0019] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0020] See also Figure 1 to Figure 2 The present invention provides the following technical solution: a hot-rolled medium manganese steel with ultra-high impact toughness and a heat treatment method thereof, wherein the medium manganese steel comprises the following components and their proportions: C: 0.04~0.43wt.%, Si: 0.36~1.40wt.%, Mn: 3.80~5.93wt.%, Al: 0.86~3.53wt.%, Nb: 0.04~0.08wt.%, Cr: 0.90~1.36wt.%, Ni: 0.85~1.65%, V: 0.11~0.19 wt.%, P≤0.010%, S≤0.002%, 0.17 wt.%≤Nb+ V≤0.25wt.%.
[0021] In this embodiment, the following specific component proportions are provided: C: 0.042wt.%, Si: 0.9wt.%, Mn: 4.80wt.%, Al: 2.5wt.%, Nb: 0.06wt.%, Cr: 1.1wt.%, Ni: 1.2%, V: 0.15 wt.%, P: 0.008%, S: 0.002%, Nb+ V: 0.22 wt.%.
[0022] This embodiment also provides the metallographic structure composition of the above-mentioned medium manganese steel: bainite + martensite: 46.5~58.8 vol.% (lath thickness 132nm), ferrite: 17.3~23.5 vol.% (lath thickness 153nm), retained austenite 23.4~30.3 vol.% (lath thickness 126nm).
[0023] This embodiment also provides the following specific heat treatment method, the steps are as follows:
[0024] S1: The processed medium manganese steel raw material is heated to 920°C, kept at this temperature for 15 minutes, and then quenched with water to room temperature;
[0025] S2, controlling the temperature to cool down to 680-750°C, and annealing at this temperature for 10 minutes;
[0026] S3, continue to control the temperature, cool it to 195-225°C and keep it warm for 12-24 hours;
[0027] S4. Air cool to room temperature.
[0028] After testing, the mechanical properties of the medium manganese steel prepared by the above method are as follows: tensile strength: 1090~1500MPa; elongation: 22.8~46.5%, elongation: 18.8~30.5%, and 20℃ V-notch impact absorption energy is 105~170J.
[0029] The above method provided by the present invention uses two-phase annealing instead of complete austenitization of the traditional process. Two-phase annealing will form lath-shaped ferrite. Since the carbon and manganese content in ferrite is extremely low, supersaturated carbon and manganese will diffuse into austenite, so that the thermal stability of austenite is enhanced. After annealing, the temperature is kept at Ms-(10~30℃) for 12~24 hours. This process is to form fine bainite. First, the austenite that is unstable at this temperature is first transformed into fine martensite. Then, as the insulation time increases, the supersaturated carbon in the martensite is partitioned into the austenite, so that the stability of the supercooled austenite is further increased, resulting in a decrease in the Ms point, and a bainite structure will be formed in the subsequent insulation process. Due to the formation of ferrite and martensite during the annealing and quenching processes, the interface between austenite and ferrite / martensite increases, providing more nucleation sites for the formation of bainite. In addition, since the bainite is formed below the Ms point of the test steel in this process, the supercooling of austenite increases, which enhances the nucleation driving force of bainite. The above reasons lead to the refinement of the bainite structure.
[0030] The refined bainite forms a layered structure with ferrite and residual austenite. When impacted, the layered structure changes the crack extension direction or passivates the crack, consumes a lot of energy, causes delayed fracture of the sample, and improves its impact toughness performance. In addition, since the stability of the residual austenite formed under this process is also greatly improved, the TRIP effect of the stable residual austenite during the impact process also consumes a lot of energy, improving the impact toughness of the steel. In addition, since the present invention contains 46.5~58.8 vol.%, and its organization is refined, this also ensures that the strength of the steel is 1090~1500MPa.
[0031] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention.
[0032] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A hot-rolled medium manganese steel with ultra-high impact toughness, characterized in that: The medium manganese steel comprises the following components and their proportions: C: 0.04-0.43wt.%, Si: 0.36-1.40wt.%, Mn: 3.80-5.93wt.%, Al: 0.86-3.53wt.%, Nb: 0.04-0.08wt.%, Cr: 0.90-1.36wt.%, Ni: 0.85-1.65%, V: 0.11-0.19 wt.%, P≤0.010%, S≤0.002%, 0.17 wt.%≤Nb+V≤0.25 wt.%, and the metallographic structure of the medium manganese steel comprises: bainite + martensite: 46.5-58.8 vol.%, ferrite: 17.3-23.5vol.%, retained austenite 23.4-30.3 vol.%, the medium manganese steel uses a heat treatment method, the heat treatment method uses two-phase zone annealing, and specifically includes the following steps: step 1, heating the processed medium manganese steel raw material to 920℃, and keeping it at this temperature, and then quenching it with water to room temperature; step 2, controlling the temperature to cool it to 680~750℃, and annealing it at this temperature; step 3, continuing to control the temperature to cool it to 195~225℃ and keeping it under this temperature adjustment; step 4, air cooling to room temperature.
2. The ultra-high impact toughness hot-rolled medium manganese steel according to claim 1, characterized in that: The medium manganese steel contains the following components and their proportions: C: 0.042wt.%, Si: 0.9wt.%, Mn: 4.80wt.%, Al: 2.5wt.%, Nb: 0.06wt.%, Cr: 1.1wt.%, Ni: 1.2%, V: 0.15 wt.%, P: 0.008%, S: 0.002%, Nb+V: 0.22 wt.%.
3. The ultra-high impact toughness hot-rolled medium manganese steel according to claim 1, characterized in that: The medium manganese steel contains the following components and their proportions: C: 0.04wt.%, Si: 0.6wt.%, Mn: 4.2wt.%, Al: 1.2wt.%, Nb: 0.05wt.%, Cr: 1.2wt.%, Ni: 1.1%, V: 0.11 wt.%, P: 0.009%, S: 0.00018%, Nb+V: 0.18wt.%.
4. A heat treatment method for preparing the medium manganese steel as claimed in claim 1, characterized in that: The heat treatment method uses two-phase zone annealing, and specifically includes the following steps: step 1, heating the processed medium manganese steel raw material to 920°C, keeping it warm at this temperature, and then quenching it with water to room temperature; step 2, controlling the temperature to cool it to 680-750°C, and annealing it at this temperature; step 3, continuing to control the temperature to cool it to 195-225°C and keeping it warm under this temperature adjustment; step 4, air cooling it to room temperature.
5. The heat treatment method according to claim 4, characterized in that: The insulation time in step 1 is 15 minutes.
6. The heat treatment method according to claim 4, characterized in that: The annealing time in step 2 is 10 min.
7. The heat treatment method according to claim 4, characterized in that: The insulation time in step 3 is 12 to 24 hours.