A heat treatment process for high speed tool steel

By adding g-C3N4 and doping B3+ during the quenching process of high-speed tool steel, and adding chlorinated paraffin to the quenching oil, the problem of high residual austenite and low hardness in high-speed tool steel is solved, and the hardness and resistance are achieved. The increase in tensile strength eliminates retained austenite and significantly improves impact toughness and surface quality.

CN118241003BActive Publication Date: 2024-10-18HUBEI HONGRUI DING TESTING TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410566083.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-10-18
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

After W4Mo2Cr4VSi and W9Mo3Cr4V high-speed tool steels are quenched by ordinary processes, the structure is martensite and granular carbide. The content of retained austenite is high and the hardness is low. It cannot meet the demand for steel for manufacturing measuring tools. There is an urgent need for a method that can reduce residual austenite. Temperature, a heat treatment process to increase hardness.

Method used

During the quenching process, g-C3N4 is added and doped with B3+ to increase the grain boundary strength, promote the formation of precipitated phases and inhibit austenite transformation. Combined with the addition of chlorinated paraffin in the quenching oil, a protective film is formed to promote austenite. Transform to martensite, lower quenching temperature, cool evenly, and reduce structural inhomogeneity.

Benefits of technology

Significantly improves the hardness and tensile strength of tool steel, eliminates retained austenite, improves impact toughness, and maintains material surface quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention proposes a heat treatment process for high-speed tool steel, comprising the following steps: S1, quenching: placing the tool steel wrapped with g-C3N4 in an air furnace, preheating to 500-650°C and then keeping it warm for 1-2h, continuing to heat to 1180-1240°C and keeping it warm at 1-1.2min / mm, and quenching after the insulation ends; S2, tempering, the tool steel after quenching in step S1 is tempered at 500-650°C for 3 times. The present invention adds g-C3N4 during quenching, thereby improving the grain boundary strength and inhibiting the austenite phase transformation, thereby improving the hardness of the tool steel and eliminating the residual austenite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tool steel, and in particular to a heat treatment process for high-speed tool steel. Background Art

[0002] High-speed tool steel is a widely used tool steel with excellent wear resistance, heat resistance and hardness. Heat treatment is a crucial step in the processing of high-speed tool steel products. Heat treatment can improve its structure and performance, and increase its hardness and wear resistance.

[0003] The heat treatment process of high-speed tool steel includes three main steps: heating, insulation and cooling. In the heating stage, high-speed tool steel products are heated to a specific temperature range to achieve the required structure and hardness. The insulation stage is to rearrange the grains inside the material to improve its strength and hardness. The cooling stage is to fix the structure of the material through rapid cooling to ensure its good performance. In practical applications, the heat treatment process of high-speed tool steel needs to be determined according to the specific material composition, shape and requirements. By reasonably designing and controlling the heat treatment process, high-speed tool steel products can achieve the best performance.

[0004] W4Mo2Cr4VSi and W9Mo3Cr4V high-speed tool steels are low-cost, have good heat treatment resistance to decarburization, small carbides, good dimensional stability, and can achieve high stability without cryogenic treatment, making them common high-speed tool steels on the market. However, after ordinary quenching treatment, W4Mo2Cr4VSi and W9Mo3Cr4V have a structure of martensite and granular carbides, a high content of retained austenite of about 8%, and a low hardness of HRC56-60, which cannot meet the steel requirements for manufacturing measuring tools. Therefore, a high-speed tool steel heat treatment process that can reduce retained austenite and increase hardness is urgently needed. Summary of the invention

[0005] In view of this, the present invention proposes a heat treatment process which can reduce the residual austenite of W4Mo2Cr4VSi and W9Mo3Cr4V and improve their hardness.

[0006] The technical solution of the present invention is implemented as follows: The present invention provides a heat treatment process for high-speed tool steel, comprising the following steps:

[0007] S1, quenching: place the tool steel wrapped with g-C3N4 in an air furnace, preheat to 500-650°C, keep warm for 1-2h, continue to heat to 1180-1240°C and keep warm at 1-1.2min / mm, and quench after the end of the warming;

[0008] S2, tempering: the tool steel after quenching in step S1 is tempered at 500-650°C for 3 times.

[0009] Adding g-C3N4 during quenching can increase the hardness of tool steel and eliminate residual austenite for the following reasons:

[0010] As a strengthening phase, g-C3N4 can form a strengthening effect at the grain boundary, hinder dislocation movement and grain boundary sliding, increase the strength and stability of the grain boundary, and thus improve the hardness of the tool steel material. In addition, during the quenching process, the addition of g-C3N4 can promote the formation of some precipitated phases (such as carbides, etc.), which can fill the grain boundaries and voids, reduce the presence of retained austenite, and thus improve the hardness of the tool steel material. The addition of g-C3N4 can also inhibit the phase transformation process from austenite to martensite during the quenching process, so that more austenite is transformed into the martensite phase, thereby eliminating the retained austenite and improving the hardness and strength of the material.

[0011] In summary, the addition of g-C3N4 can improve the hardness of tool steel and eliminate retained austenite by improving grain boundary strength, promoting the formation of precipitate phase and inhibiting austenite transformation.

[0012] On the basis of the above technical solution, preferably, the g-C3N4 doped with B 3+ .

[0013] Specifically, g-C3N4 and B 3+ Doping can introduce lattice defects, such as point defects and dislocations, which can promote the nucleation and growth of the martensite phase, and are beneficial to the transformation of austenite to martensite in tool steel, thereby improving the hardness of tool steel. 3+ As a solid solution strengthening element, it can enhance the solid solution strengthening effect in tool steel and improve the tensile strength and hardness of steel. The doping of g-C3N4 can increase the strength and stability of grain boundaries and further improve the hardness of tool steel.

[0014] In summary, g-C3N4 doped with B 3+ The hardness of tool steel can be improved and residual austenite can be eliminated through lattice defect regulation and solid solution strengthening mechanism.

[0015] On the basis of the above technical solution, preferably, the g-C3N4 doped with B 3+ The preparation method is as follows: melamine and borax are ground and mixed, calcined at 500-600°C for 3-5h, then cooled to room temperature, ground, washed, centrifuged, and dried to obtain doped B 3+ of g-C3N4.

[0016] On the basis of the above technical solution, preferably, the molar ratio of melamine:borax is 1:(0.01-0.05).

[0017] On the basis of the above technical solution, preferably, oil quenching is adopted in step S1, and the components of the quenching oil are No. 10 machine oil and chlorinated paraffin.

[0018] Specifically, chlorinated paraffin can increase the surface tension of quenching oil, making it easier for tool steel to form a uniform cooling rate distribution during the quenching process, which is conducive to reducing organizational heterogeneity and improving the hardness and strength of tool steel materials. The chloride ions in chlorinated paraffin can promote the transformation of austenite to martensite during the quenching process. The chloride ions can cause local stress concentration near grain boundaries and dislocations, thereby promoting the nucleation and growth of martensite and improving the hardness of tool steel. The carbon element in chlorinated paraffin can combine with the iron element in steel during the quenching process to form carbides, which can fill grain boundaries and voids, enhance the strength of grain boundaries, and improve the hardness and strength of tool steel.

[0019] In addition, chlorinated paraffin can absorb heat during the quenching process, reduce the quenching temperature, and make the quenching temperature of tool steel more uniform and stable, which helps to reduce deformation and cracks and improve the strength and hardness of the material. Chlorinated paraffin can also form a protective film during the quenching process to prevent oxidation and decarburization on the surface of tool steel and maintain the surface quality and hardness of the material.

[0020] On the basis of the above technical solution, preferably, the addition amount of the chlorinated paraffin is 1 wt% to 3 wt%.

[0021] On the basis of the above technical scheme, preferably, the tempering treatment method in step S2 is: the first tempering temperature is 500-650°C, and the ice-water mixture is cooled after keeping warm for 2-3 hours; the second and third tempering temperatures are 500-600°C, and the low-temperature nitrogen is cooled after keeping warm for 2-3 hours.

[0022] On the basis of the above technical solution, preferably, the chemical formula of the tool steel raw material is one of W4Mo2Cr4VSi and W9Mo3Cr4V.

[0023] On the basis of the above technical scheme, preferably, the W4Mo2Cr4VSi component includes the following raw materials in weight percentage: C 0.7%-0.8%, Si 0.8%-1.3%, Mn 0.2%-0.4%, Cr 3.8%-4.4%, V 0.5%-1.0%, Mo 0.5%-1.2%, W 1.5%-2.5%, and the balance is Fe.

[0024] On the basis of the above technical scheme, preferably, the W9Mo3Cr4V component includes the following raw materials in weight percentage: C 0.77%-0.85%, Si 0.2%-0.4%, Mn 0.2%-0.4%, Cr 3.6%-4.2%, V 1.3%-1.6%, Mo 2.7%-3.3%, W 8.5%-9.5%, and the balance is Fe.

[0025] The heat treatment process of a high-speed tool steel of the present invention has the following beneficial effects compared with the prior art:

[0026] (1) The present invention adds g-C3N4 during quenching, which has the technical effects of improving grain boundary strength, promoting the formation of precipitation phase and inhibiting austenite phase transformation, improving the hardness of tool steel, and eliminating residual austenite.

[0027] (2) The present invention involves doping B in g-C3N4 3+ It plays a role in increasing the temperature resistance of g-C3N4, preventing it from decomposing at high temperatures and improving the quenching effect; at the same time, doping B 3+ It is also beneficial to the transformation of austenite to martensite in tool steel, thereby increasing the hardness of tool steel.

[0028] (3) The present invention improves the strength and hardness of tool steel by adding chlorinated paraffin to quenching oil, and also has the technical effect of preventing oxidation and decarburization of the steel surface. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The W4Mo2Cr4VSi and W9Mo3Cr4V high-speed tool steels used in the present invention are both purchased from Shanghai Weili Group, wherein the W4Mo2Cr4VSi composition includes the following raw materials in weight percentage: C 0.7%-0.8%, Si 0.8%-1.3%, Mn 0.2%-0.4%, Cr 3.8%-4.4%, V 0.5%-1.0%, Mo 0.5%-1.2%, W 1.5%-2.5%, and the balance is Fe. The W9Mo3Cr4V composition includes the following raw materials in weight percentage: C 0.77%-0.85%, Si 0.2%-0.4%, Mn 0.2%-0.4%, Cr 3.6%-4.2%, V 1.3%-1.6%, Mo 2.7%-3.3%, W 8.5%-9.5%, and the balance is Fe.

[0031] Example 1

[0032] The heat treatment process of the W4Mo2Cr4VSi high speed tool steel of this embodiment comprises the following steps:

[0033] S1, quenching: g-C3N4 is attached to the surface of tool steel W4Mo2Cr4VSi in the form of powder spraying with a thickness of 50μm. Then the tool steel wrapped with g-C3N4 is placed in an air furnace, preheated to 500℃ and kept warm for 2h, and then heated to 1200℃ and kept warm at 1.2min / mm. After the insulation is completed, it is quenched with No. 10 mechanical oil.

[0034] The preparation method of g-C3N4 is as follows: melamine is ground and calcined at 500°C for 5h, then cooled to room temperature for grinding, washed, centrifuged and dried to obtain g-C3N4.

[0035] S2, tempering, the first tempering temperature is 500℃, kept warm for 3h and then cooled with ice-water mixture; the second tempering temperature is 550℃, kept warm for 3h and then cooled with low-temperature nitrogen; the third tempering temperature is 500℃, kept warm for 2h and then cooled with low-temperature nitrogen.

[0036] The raw material composition of W4Mo2Cr4VSi tool steel includes the following raw materials in weight percentage: C 0.75%, Si 0.8%, Mn 0.2%, Cr 4.1%, V 0.8%, Mo 0.5%, W 2.1%, and the balance is Fe.

[0037] Example 2

[0038] The heat treatment process of the W4Mo2Cr4VSi high speed tool steel of this embodiment comprises the following steps:

[0039] S1, quenching: doping B 3+The g-C3N4 was attached to the surface of tool steel W4Mo2Cr4VSi by powder spraying with a thickness of 50μm, and then the B-doped 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 500°C and kept warm for 2 hours, then heated to 1200°C and kept warm at 1.2min / mm. After the insulation, it was quenched with No. 10 mechanical oil.

[0040] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.01, calcined at 500°C for 5h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain the doped B 3+ of g-C3N4.

[0041] S2, tempering, the first tempering temperature is 500℃, kept warm for 3h and then cooled with ice-water mixture; the second tempering temperature is 550℃, kept warm for 3h and then cooled with low-temperature nitrogen; the third tempering temperature is 500℃, kept warm for 2h and then cooled with low-temperature nitrogen.

[0042] The raw material composition of W4Mo2Cr4VSi tool steel includes the following raw materials in weight percentage: C 0.75%, Si 0.8%, Mn 0.2%, Cr 4.1%, V 0.8%, Mo 0.5%, W 2.1%, and the balance is Fe.

[0043] Example 3

[0044] The heat treatment process of the W4Mo2Cr4VSi high speed tool steel of this embodiment comprises the following steps:

[0045] S1, quenching: doping B 3+ The g-C3N4 was attached to the surface of tool steel W4Mo2Cr4VSi by powder spraying with a thickness of 50μm, and then the B-doped 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 500°C and kept warm for 2 hours, then heated to 1200°C and kept warm at 1.2 min / mm. After the insulation, it was oil quenched by adding 1 wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0046] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.01, calcined at 500°C for 5h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain the doped B 3+ of g-C3N4.

[0047] S2, tempering, the first tempering temperature is 500℃, kept warm for 3h and then cooled with ice-water mixture; the second tempering temperature is 550℃, kept warm for 3h and then cooled with low-temperature nitrogen; the third tempering temperature is 500℃, kept warm for 2h and then cooled with low-temperature nitrogen.

[0048] The raw material composition of W4Mo2Cr4VSi tool steel includes the following raw materials in weight percentage: C 0.75%, Si 0.8%, Mn 0.2%, Cr 4.1%, V 0.8%, Mo 0.5%, W 2.1%, and the balance is Fe.

[0049] Example 4

[0050] The heat treatment process of the W4Mo2Cr4VSi high speed tool steel of this embodiment comprises the following steps:

[0051] S1, quenching: doping B 3+ The g-C3N4 was attached to the surface of tool steel W4Mo2Cr4VSi by powder spraying with a thickness of 50μm, and then the B-doped 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 650°C and kept warm for 1h, then heated to 1240°C and kept warm at 1.2min / mm. After the insulation, it was oil quenched by adding 3wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0052] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.05, calcined at 600°C for 3h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain doped B 3+ of g-C3N4.

[0053] S2, tempering, the first tempering temperature is 650℃, kept warm for 2h and then cooled with ice-water mixture; the second tempering temperature is 600℃, kept warm for 2h and then cooled with low-temperature nitrogen; the third tempering temperature is 550℃, kept warm for 3h and then cooled with low-temperature nitrogen.

[0054] The raw material composition of W4Mo2Cr4VSi tool steel includes the following raw materials in weight percentage: C 0.7%, Si 1.1%, Mn 0.3%, Cr 3.8%, V 0.5%, Mo 0.9%, W 1.5%, and the balance is Fe.

[0055] Example 5

[0056] The heat treatment process of the W4Mo2Cr4VSi high speed tool steel of this embodiment comprises the following steps:

[0057] S1, quenching: doping B 3+The g-C3N4 was attached to the surface of tool steel W4Mo2Cr4VSi by powder spraying with a thickness of 50μm, and then the B-doped 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 550°C and kept warm for 2 hours, then heated to 1220°C and kept warm at 1.2 min / mm. After the insulation, it was oil quenched by adding 2 wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0058] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.03, calcined at 550°C for 4h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain doped B 3+ of g-C3N4.

[0059] S2, tempering, the first tempering temperature is 650℃, kept warm for 3h and then cooled with ice-water mixture; the second tempering temperature is 600℃, kept warm for 3h and then cooled with low-temperature nitrogen; the third tempering temperature is 600℃, kept warm for 2h and then cooled with low-temperature nitrogen.

[0060] The raw material composition of W4Mo2Cr4VSi tool steel includes the following raw materials in weight percentage: C 0.8%, Si 1.3%, Mn 0.4%, Cr 4.4%, V 1.0%, Mo 1.2%, W 2.5%, and the balance is Fe.

[0061] Example 6

[0062] The heat treatment process of the W9Mo3Cr4V high speed tool steel of this embodiment comprises the following steps:

[0063] S1, quenching: doping B 3+ The g-C3N4 was attached to the surface of tool steel W9Mo3Cr4V by powder spraying with a thickness of 50μm, and then the doped B 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 550°C and kept warm for 1.5h, then heated to 1180°C and kept warm at 1.0min / mm. After the insulation, it was oil quenched by adding 2wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0064] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.03, calcined at 500°C for 5h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain the doped B 3+ of g-C3N4.

[0065] S2, tempering, the first tempering temperature is 540℃, and it is cooled with ice-water mixture after keeping warm for 3 hours; the second tempering temperature is 550℃, and it is cooled with low-temperature nitrogen after keeping warm for 3 hours; the third tempering temperature is 550℃, and it is cooled with low-temperature nitrogen after keeping warm for 2 hours.

[0066] The raw material composition of W9Mo3Cr4V tool steel includes the following raw materials in weight percentage: C 0.81%, Si 0.4%, Mn0.2%, Cr 3.9%, V 1.6%, Mo 2.7%, W 8.5%, and the balance is Fe.

[0067] Example 7

[0068] The heat treatment process of the W9Mo3Cr4V high speed tool steel of this embodiment comprises the following steps:

[0069] S1, quenching: doping B 3+ The g-C3N4 was attached to the surface of tool steel W9Mo3Cr4V by powder spraying with a thickness of 50μm, and then the doped B 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 630°C and kept warm for 1h, then heated to 1220°C and kept warm at 1.0min / mm. After the insulation, it was oil quenched by adding 3wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0070] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.05, calcined at 550°C for 4 hours, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain doped B 3+ of g-C3N4.

[0071] S2, tempering, the first tempering temperature is 630℃, kept warm for 2h and then cooled with ice-water mixture; the second tempering temperature is 600℃, kept warm for 3h and then cooled with low-temperature nitrogen; the third tempering temperature is 550℃, kept warm for 2h and then cooled with low-temperature nitrogen.

[0072] The raw material composition of W9Mo3Cr4V tool steel includes the following raw materials in weight percentage: C 0.77%, Si 0.3%, Mn 0.4%, Cr 4.2%, V 1.3%, Mo 3.3%, W 9.0%, and the balance is Fe.

[0073] Example 8

[0074] The heat treatment process of the W9Mo3Cr4V high speed tool steel of this embodiment comprises the following steps:

[0075] S1, quenching: doping B 3+The g-C3N4 was attached to the surface of tool steel W9Mo3Cr4V by powder spraying with a thickness of 50μm, and then the doped B 3+ The g-C3N4 tool steel was placed in an air furnace, preheated to 500°C and kept warm for 2 hours, then heated to 1180°C and kept warm at 1.0 min / mm. After the insulation, it was oil quenched by adding 1 wt% of chlorinated paraffin to No. 10 machine oil during quenching.

[0076] Doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed in a molar ratio of melamine to borax of 1:0.01, calcined at 500°C for 5h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain the doped B 3+ of g-C3N4.

[0077] S2, tempering, the first tempering temperature is 600℃, and it is cooled with ice-water mixture after keeping warm for 2.5h; the second tempering temperature is 600℃, and it is cooled with low-temperature nitrogen after keeping warm for 2h; the third tempering temperature is 550℃, and it is cooled with low-temperature nitrogen after keeping warm for 2h.

[0078] The raw material composition of W9Mo3Cr4V tool steel includes the following raw materials in weight percentage: C 0.85%, Si 0.2%, Mn0.3%, Cr 3.6%, V 1.5%, Mo 3.0%, W 9.5%, and the balance is Fe.

[0079] Comparative Example 1

[0080] The difference between Comparative Example 1 and Example 1 is that the process is directly quenched and g-C3N4 is not wrapped. The rest of the contents are the same as Example 1.

[0081] Comparative Example 2

[0082] The difference between Comparative Example 2 and Example 1 is that the quenching temperature is lower, specifically, preheating to 500° C. and then keeping the temperature for 2 hours, and then continuing to heat to 1000° C. and keeping the temperature at 1.2 min / mm. The rest of the contents are the same as Example 1.

[0083] Comparative Example 3

[0084] The difference between Comparative Example 3 and Example 1 is that the tempering temperature is lower, specifically, the first tempering temperature is 400°C, and the ice-water mixture is cooled after keeping warm for 3 hours; the second tempering temperature is 450°C, and the low-temperature nitrogen is cooled after keeping warm for 3 hours; the third tempering temperature is 300°C, and the low-temperature nitrogen is cooled after keeping warm for 2 hours. The rest of the contents are the same as Example 1.

[0085] Comparative Example 4

[0086] The difference between Comparative Example 4 and Example 1 is that tempering is performed only once, specifically: the tempering temperature is 500° C., and the mixture is cooled with ice and water after being kept warm for 3 hours. The rest of the contents are the same as Example 1.

[0087] Comparative Example 5

[0088] The difference between Comparative Example 5 and Example 2 is that the molar ratio of melamine:borax is 1:0.1, and the amount of borax exceeds the specified range of this application. The rest of the contents are the same as Example 2.

[0089] Comparative Example 6

[0090] The difference between Comparative Example 6 and Example 3 is that 5 wt % of chlorinated paraffin is added to No. 10 machine oil during quenching, and the amount of chlorinated paraffin exceeds the specified range of this application. The rest of the contents are the same as Example 3.

[0091] Table 1 Hardness and austenite of tool steel after heat treatment

[0092] Hardness(HRC) Retained austenite(%) <![CDATA[Impact toughness αk (J / cm 2 )]]> Example 1 64 1.3 49 Example 2 66 0.8 55 Example 3 70 0.1 59 Example 4 71 0.2 61 Example 5 72 0.1 63 Example 6 72 0.1 65 Example 7 71 0.1 63 Example 8 70 0.1 62 Comparative Example 1 61 5.6 35 Comparative Example 2 62 4.7 38 Comparative Example 3 62 4.3 37 Comparative Example 4 61 4.1 37 Comparative Example 5 62 3.8 41 Comparative Example 6 62 3.4 42

[0093] As shown in Table 1, the hardness and impact toughness of the tool steel after heat treatment in the embodiment of the present invention are significantly improved, and the retained austenite is significantly reduced, which proves that the g-C3N4 is wrapped during quenching and the B is doped. 3+ g-C3N4, adding chlorinated paraffin to quenching oil has a positive effect on hardness, impact toughness and retained austenite. It can be seen from the comparative example that quenching temperature, tempering temperature, tempering times, and the addition amount of borax and chlorinated paraffin will have a direct impact on the hardness, impact toughness and retained austenite of tool steel. Based on the above analysis, it is concluded that the treatment process of Example 6 is the best.

[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A heat treatment process for high speed tool steel, characterized in that: The following steps are involved: S1, quenching: wrap the doped B 3+ The g-C3N4 tool steel is placed in an air furnace, preheated to 500-650°C, kept warm for 1-2 hours, and then heated to 1180-1240°C at a temperature of 1-1.2 min / mm. After the end of the heat preservation, quenching is performed. S2, tempering, the tool steel after quenching in step S1 is tempered at 500-650°C for 3 times; The doped B 3+ The preparation method of g-C3N4 is as follows: melamine and borax are ground and mixed, calcined at 500-600°C for 3-5h, then cooled to room temperature for grinding, washed, centrifuged, and dried to obtain doped B 3+ g-C3N4; The tool steel is W4Mo2Cr4VSi or W9Mo3Cr4V.

2. A heat treatment process for high speed tool steel according to claim 1, characterized in that: The molar ratio of melamine to borax is 1:(0.01-0.05).

3. The heat treatment process for high speed tool steel according to claim 1, characterized in that: In step S1, oil quenching is adopted, and the components of the quenching oil are No. 10 machine oil and chlorinated paraffin.

4. A heat treatment process for high speed tool steel as claimed in claim 3, characterized in that: The addition amount of the chlorinated paraffin is 1 wt% to 3 wt%.

5. The heat treatment process for high speed tool steel according to claim 1, characterized in that: The tempering treatment method in step S2 is: the first tempering temperature is 500-650° C., and the mixture is cooled with ice and water after being kept warm for 2-3 hours; the second and third tempering temperatures are 500-600° C., and the mixture is cooled with nitrogen after being kept warm for 2-3 hours.

6. A heat treatment process for high speed tool steel according to claim 1, characterized in that: The W4Mo2Cr4VSi composition includes the following raw materials in weight percentage: C 0.7%-0.8%, Si 0.8%-1.3%, Mn 0.2%-0.4%, Cr3.8%-4.4%, V 0.5%-1.0%, Mo 0.5%-1.2%, W 1.5%-2.5%, and the balance is Fe.

7. The heat treatment process for high speed tool steel according to claim 1, characterized in that: The W9Mo3Cr4V composition includes the following raw materials in weight percentage: C 0.77%-0.85%, Si 0.2%-0.4%, Mn 0.2%-0.4%, Cr3.6%-4.2%, V 1.3%-1.6%, Mo 2.7%-3.3%, W 8.5%-9.5%, and the balance is Fe.

Citation Information

Patent Citations

  • Manufacturing method of file for special tool inspection

    CN110004284A

  • Aluminum alloy stamping die steel and preparation method thereof

    CN116891978A