A 4-series aluminum alloy and its preparation method and application

By adding Re and Y to the aluminum alloy to form clusters, and adding CeO2, combined with specific heat treatment steps, the problem of cracks and performance imbalance in the 4 series aluminum alloy during the casting process is solved, and excellent mechanical properties and performance are achieved. Corrosion resistance improves the overall performance of aluminum alloys.

CN118241082BActive Publication Date: 2024-10-25福建祥鑫新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410263989.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-07
Publication Date
2024-10-25
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

Existing 4 series aluminum alloys are prone to cracks during the casting process, and it is difficult to achieve a balance between mechanical properties and corrosion resistance, which affects their application.

Method used

By adding Re and Y to the aluminum alloy to form Re- and Y-rich clusters to hinder the growth of the eutectic Si phase, and adding CeO2 to improve the electrochemical properties, combined with specific heat treatment steps, we can prepare an alloy with excellent mechanical properties and durability. Corrosion resistant 4 series aluminum alloy.

Benefits of technology

There are no cracks inside the aluminum alloy, the mechanical properties are improved, the corrosion resistance is improved, and the hardness is improved, which solves the problems in the existing technology that aluminum alloys are prone to cracks and have unbalanced properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118241082B_ABST
    Figure CN118241082B_ABST
Patent Text Reader

Abstract

The present invention provides a 4-series aluminum alloy and a preparation method and application thereof, wherein the 4-series aluminum alloy comprises the following components in mass percentage: Si 10.0-11.5%, Fe 0.50%, Cu 2.0-3.0%, Mn 0.10%, Mg 0.20-0.50%, Ni 0.30%, Zn 0.30%, Ti 0.10%, Re 0.1-0.3%, Y 0.05-0.1%, CeO 2 0.1-0.15%, other single impurity elements ≤ 0.05%, total impurity content ≤ 0.15%, and the remainder is Al. The mass ratio of Re to Y is 2-4:1; the average particle size of CeO 2 is 20-50nm, and the specific surface area is 40-70m 2 / g. The present invention combines component design with a preparation method, so that the aluminum alloy has excellent mechanical properties, good corrosion resistance, and no cracks inside the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum alloy preparation, and in particular relates to a 4 series aluminum alloy and a preparation method and application thereof. Background Art

[0002] Aluminum has been used in the construction industry for more than 100 years. It was first used as a building decoration material, such as door and window frames, glass curtain wall frames, building exterior aluminum panels, and building vertical lock seam roofs. In the 1930s, aluminum alloys were used in the load-bearing and maintenance structures of buildings; today, aluminum alloys have become the largest building metal material besides steel. Aluminum alloys are the most widely used type of metal structural materials in industry, and have been widely used in aviation, aerospace, automobiles, machinery manufacturing, shipbuilding and chemical industries. Aluminum alloys can be divided into two categories: forged aluminum and cast aluminum. The former is the hot working or cold working of unmelted aluminum billets, and the latter is the pouring of molten aluminum into a mold and then casting it. The commonly used aluminum alloy for structures is forged aluminum. The forged aluminum alloy grade is usually represented by a four-digit number. The strength, ductility, corrosion resistance and other properties of forged aluminum alloys of different grades vary due to differences in their chemical composition content.

[0003] 4 series aluminum alloys belong to the series with high silicon content and can be used for building materials, mechanical parts, forging materials, etc. However, in the prior art, due to the stress concentration inside the material during the casting process of the existing 4 series aluminum alloy rods, especially the 4 series aluminum alloy rods with smaller diameters, cracks are generated. In addition, if the temperature control during the manufacturing process is improper or the cooling speed is too fast, it will also lead to the formation of central cracks in the aluminum alloy round rods. At the same time, it is difficult to achieve a balance between mechanical properties and corrosion resistance, which directly affects the application of 4 series aluminum alloys. Therefore, a 4 series aluminum alloy and a preparation method thereof are urgently needed to solve the problems existing in the existing 4 series aluminum alloy production. Summary of the invention

[0004] The purpose of the present invention is to provide a 4 series aluminum alloy and a preparation method thereof. By combining component design and preparation method, the obtained aluminum alloy has excellent mechanical properties, good corrosion resistance and no internal crack problem.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A 4 series aluminum alloy comprises the following components in mass percentage: Si 10.0-11.5%, Fe 0.50%, Cu 2.0-3.0%, Mn 0.10%, Mg 0.20-0.50%, Ni 0.30%, Zn 0.30%, Ti 0.10%, Re 0.1-0.3%, Y 0.05-0.1%, CeO 2 0.1-0.15%, other single impurity elements ≤ 0.05%, total impurity content ≤ 0.15%, and the balance is Al.

[0007] Furthermore, the mass ratio of Re to Y is 2-4:1.

[0008] The present invention can improve the mechanical properties of aluminum alloys by adding Re and Y. It is speculated that the addition of these two elements can form clusters rich in Re and Y, which are adsorbed on the growth steps of the eutectic Si phase, hindering the eutectic Si phase from growing from the steps to coarse and brittle lamellar shapes, and at the same time, a large number of fine particles can be formed in the Al-Si melt, further hindering the growth of the eutectic Si phase, thereby improving the mechanical properties of the aluminum alloy. The inventor unexpectedly discovered that when the mass ratio of Re and Y is 2-4:1, the interior of the obtained aluminum alloy is crack-free. It is speculated that under this condition, the difference in grain size inside the aluminum alloy is smaller, the phase distribution is uniform, and a more uniform organizational structure is formed inside the aluminum alloy. The present invention selects Re and Y to add synergistically, thereby efficiently and synergistically strengthening the fine grain strengthening effect of the α-Al phase and the modification strengthening and toughening effect of the eutectic Si phase.

[0009] Furthermore, the average particle size of the CeO2 is 20-50nm.

[0010] Furthermore, the specific surface area of ​​CeO2 is 40-70m 2 / g.

[0011] The addition of Re and Y to the aluminum alloy of the present invention can improve its mechanical properties, but the addition of Re and Y may have a negative impact on the corrosion resistance of the aluminum alloy. It is speculated that the presence of Re and Y will increase the electrochemical activity of the aluminum alloy, making it more susceptible to electrochemical corrosion, and the interaction with other elements may also reduce the corrosion resistance of some elements in the alloy, thereby reducing the corrosion resistance of the aluminum alloy. In order to improve the corrosion resistance of the aluminum alloy, the present invention adds CeO2 to reduce the maximum intergranular corrosion depth of the aluminum alloy. It is speculated that the presence of CeO2 can change the electrochemical properties of the aluminum alloy, inhibit the electrochemical reaction between the metal and the corrosive medium, and slow down the development speed of intergranular corrosion, thereby reducing the maximum intergranular corrosion depth. By selecting a suitable particle size and specific surface area of ​​CeO2, the corrosion resistance of the aluminum alloy can be more significantly improved. The inventor also unexpectedly discovered that under this condition, the hardness of the aluminum alloy can also be improved.

[0012] The present invention provides a method for preparing a 4-series aluminum alloy, comprising the following steps:

[0013] (1) Weighing raw materials according to the mass percentage of aluminum alloy components;

[0014] (2) melting the weighed raw materials at 660-670° C., heating to 740-750° C., adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid;

[0015] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0016] (4) The cast rod is subjected to T6 heat treatment to obtain a 4 series aluminum alloy.

[0017] Furthermore, the refining agent is 65wt% Na2SiF6+35wt% C2Cl6.

[0018] Furthermore, the amount of the refining agent added is 0.25% of the total mass of the raw material.

[0019] Furthermore, the T6 heat treatment is specifically 500□510℃ solution treatment for 2□4h; 70□75℃ hot water quenching for 5□10min; 170□180℃ aging treatment for 14□16h.

[0020] Furthermore, the T6 heat treatment is specifically solution treatment at 505° C. for 3 hours; hot water quenching at 72° C. for 8 minutes; and aging treatment at 175° C. for 15 hours.

[0021] The present invention also provides an application of a 4-series aluminum alloy.

[0022] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0023] 1. The present invention provides a 4 series aluminum alloy and a preparation method thereof. By combining component design and preparation method, the obtained aluminum alloy has excellent mechanical properties and good corrosion resistance. The produced aluminum alloy rod has no cracks inside. In particular, it can solve the problem of easy cracking in directly preparing 4 series aluminum alloy rods with smaller diameters in the prior art, and at the same time can achieve excellent mechanical properties and corrosion resistance.

[0024] 2. The present invention can improve the mechanical properties of aluminum alloys by adding Re and Y. At the same time, when the mass ratio of Re to Y is 2-4:1, there is no crack inside the obtained aluminum alloy. It is speculated that under this condition, the difference in grain size inside the aluminum alloy is smaller, the phase distribution is uniform, and a more uniform organizational structure is formed inside the aluminum alloy. The present invention selects Re and Y to be added synergistically, thereby efficiently and synergistically strengthening the fine grain strengthening effect of the α-Al phase and the modification strengthening and toughening effect of the eutectic Si phase.

[0025] 3. Adding Re and Y to the aluminum alloy of the present invention can improve its mechanical properties, but the addition of Re and Y may have a negative impact on the corrosion resistance of the aluminum alloy. In order to improve the corrosion resistance of the aluminum alloy, the present invention adds CeO2 to reduce the maximum intergranular corrosion depth of the aluminum alloy. By selecting a suitable particle size and specific surface area of ​​CeO2, the corrosion resistance of the aluminum alloy can be more significantly improved. The inventors also unexpectedly found that under this condition, the hardness of the aluminum alloy can also be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the macrostructure of the aluminum alloy prepared in the present invention, wherein the left figure is the aluminum alloy prepared in Example 1, and the right figure is the aluminum alloy prepared in Example 2;

[0027] Figure 2 Schematic diagram of microstructure detection of aluminum alloy prepared in the present invention, wherein the left figure (A, a) is the aluminum alloy prepared in Example 1, and the right figure (B, b) is the aluminum alloy prepared in Example 2;

[0028] Figure 3 A schematic diagram of an aluminum alloy product prepared by the present invention;

[0029] Figure 4 It is a schematic diagram of a workpiece prepared using the aluminum alloy of the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] The present embodiment provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.17%, Y0.07%, CeO20.12%, the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0033] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0034] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0035] (1) Weigh the raw materials according to mass percentage;

[0036] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0037] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0038] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0039] Example 2

[0040] The present embodiment provides a 4 series aluminum alloy, including the following components in mass percentage: Si 10.0%, Fe 0.50%, Cu 2.0%, Mn 0.10%, Mg 0.20%, Ni 0.30%, Zn 0.30%, Ti 0.10%, Re 0.1%, Y 0.05%, CeO 2 0.1%, and the remaining individual impurity elements ≤ 0.05%, the total impurity content ≤ 0.15%, and the balance is Al.

[0041] The average particle size of CeO2 is 20-50nm, and the specific surface area of ​​CeO2 is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0042] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0043] (1) Weigh the raw materials according to mass percentage;

[0044] (2) melting the weighed raw materials at 660° C., heating to 740° C., adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid;

[0045] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0046] (4) The cast rod is subjected to T6 heat treatment to obtain a 4 series aluminum alloy.

[0047] The refining agent is 65wt% Na2SiF6+35wt% C2Cl6.

[0048] The amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0049] The T6 heat treatment specifically includes solution treatment at 500° C. for 2 h, hot water quenching at 70° C. for 5 min, and aging treatment at 170° C. for 14 h.

[0050] Example 3

[0051] The present embodiment provides a 4 series aluminum alloy, including the following components in mass percentage: Si11.5%, Fe0.50%, Cu3.0%, Mn0.10%, Mg0.50%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.2%, Y0.05%, CeO20.15%, the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0052] The average particle size of CeO2 is 20-50nm. The specific surface area of ​​CeO2 is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0053] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0054] (1) Weigh the raw materials according to mass percentage;

[0055] (2) The weighed raw materials are melted at 670°C, heated to 750°C, and a refining agent is added under a nitrogen atmosphere. The mixture is refined for 30 minutes to obtain refined aluminum liquid; the refining agent is 65wt% Na2SiF6+35wt% C2Cl6, and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0056] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0057] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 510°C for 4 hours, hot water quenching at 75°C for 10 minutes, and aging treatment at 180°C for 16 hours to obtain a 4 series aluminum alloy.

[0058] Comparative Example 1

[0059] The difference between this comparative example and Example 1 is that the aluminum alloy does not include Re.

[0060] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Y0.07%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0061] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0062] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0063] (1) Weigh the raw materials according to mass percentage;

[0064] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0065] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0066] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0067] Comparative Example 2

[0068] The difference between this comparative example and Example 1 is that Y is not included in the aluminum alloy.

[0069] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.17%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0070] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0071] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0072] (1) Weigh the raw materials according to mass percentage;

[0073] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0074] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0075] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0076] Comparative Example 3

[0077] The difference between this comparative example and Example 1 is that CeO2 is not included in the aluminum alloy.

[0078] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.17%, Y0.07%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0079] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0080] (1) Weigh the raw materials according to mass percentage;

[0081] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0082] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0083] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0084] Comparative Example 4

[0085] The difference between this comparative example and Example 1 is that the mass ratio of Re to Y is 1:1.

[0086] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.1%, Y0.1%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0087] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0088] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0089] (1) Weigh the raw materials according to mass percentage;

[0090] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0091] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0092] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0093] Comparative Example 5

[0094] The difference between this comparative example and Example 1 is that the mass ratio of Re to Y is 5:1.

[0095] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.25%, Y0.05%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0096] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0097] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0098] (1) Weigh the raw materials according to mass percentage;

[0099] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0100] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0101] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0102] Comparative Example 6

[0103] The difference between this comparative example and Example 1 is that the particle size and specific surface area of ​​CeO2 are changed.

[0104] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu2.6%, Mn0.10%, Mg0.35%, Ni0.30%, Zn0.30%, Ti0.10%, Re0.17%, Y0.07%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0105] The average particle size of CeO2 is 50-100nm, and the specific surface area is 90-150m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0106] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0107] (1) Weigh the raw materials according to mass percentage;

[0108] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0109] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0110] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0111] Comparative Example 7

[0112] The difference between this comparative example and Example 1 is that the mass percentages of some components are changed.

[0113] Specifically: This comparative example provides a 4 series aluminum alloy, including the following components in mass percentage: Si10.6%, Fe0.50%, Cu1.5%, Mn0.05%, Mg1.55%, Ni0.30%, Zn0.35%, Ti0.10%, Re0.17%, Y0.07%, CeO20.12%, and the remaining individual impurity elements ≤0.05%, the total impurity content ≤0.15%, and the balance is Al.

[0114] The average particle size of CeO2 is 20-50nm, and the specific surface area is 40-70m 2 / g. Purchased from Angxing New Carbon Materials Changzhou Co., Ltd.

[0115] The preparation method of the 4 series aluminum alloy comprises the following steps:

[0116] (1) Weigh the raw materials according to mass percentage;

[0117] (2) Melting the weighed raw materials at 665°C, heating to 745°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; wherein the refining agent is 65wt% Na2SiF6+35wt% C2Cl6; and the amount of the refining agent added is 0.25% of the total mass of the raw materials.

[0118] (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and cooling with 120 tons / h of cooling water to obtain a cast rod;

[0119] (4) The cast rod is subjected to T6 heat treatment, which specifically includes solution treatment at 505°C for 3 h; hot water quenching at 72°C for 8 min; and aging treatment at 175°C for 15 h to obtain a 4 series aluminum alloy.

[0120] Performance Testing

[0121] The diameter of the aluminum alloys prepared in Examples 1-3 and Comparative Examples 1-7 was 80 mm, and performance tests were performed.

[0122] 1. The mechanical properties of the aluminum alloys prepared in Examples 1-3 and Comparative Examples 1-7 were measured with reference to GB / T228-2002 at a temperature of 23°C. The results are shown in Table 1.

[0123] Table 1 Mechanical test results

[0124]

[0125] 2. The maximum intergranular corrosion depth of the aluminum alloys prepared in Examples 1-3 and Comparative Examples 1-7 was determined with reference to GB / T7998□2005, as shown in Table 2.

[0126] Table 2 Maximum intergranular corrosion depth

[0127]

[0128] 4. Referring to YS / T67-2012 and GB / T3191-2010, the macrostructure of the aluminum alloys of Examples 1-3 and Comparative Examples 1-7 was evaluated. The results are shown in Table 3.

[0129]

[0130]

[0131] like Figure 1 As shown, the aluminum alloy test surface prepared by the present invention has no cracks, looseness, shrinkage tails, no bright grains, no non-metallic inclusions, no stratification, and the maximum depth of the coarse grain ring of the sample is 0.5mm.

[0132] 5. With reference to YS / T67-2012 and GB / T3191-2010, the aluminum alloy samples of Examples 1-2 were tested for microstructure, sintering and primary silicon. After inspection, all samples were found to be unsintered, and the size of primary silicon was less than 0.05 μm. Figure 2 .

[0133] It can be seen from Examples 1-2 that the aluminum alloy prepared by the present invention has excellent comprehensive performance. The aluminum alloy products prepared by the present invention are as follows: Figure 3 As shown, the aluminum alloy prepared by the present invention can be applied to multiple application fields. Figure 4 For the processed parts prepared by using the aluminum alloy of the present invention, the annual output of the method of the present invention can reach 500 tons / year, which has important economic value.

[0134] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A 4 series aluminum alloy, characterized in that: The invention comprises the following components in mass percentage: Si 10.0-11.5%, Fe 0.50%, Cu 2.0-3.0%, Mn 0.10%, Mg 0.20-0.50%, Ni 0.30%, Zn 0.30%, Ti 0.10%, Re 0.1-0.3%, Y 0.05-0.1%, CeO 2 0.1-0.15%, other single impurity elements ≤ 0.05%, total impurity content ≤ 0.15%, and the balance is Al; the mass ratio of Re to Y is 2-4:

1.

2. A 4 series aluminum alloy according to claim 1, characterized in that: The average particle size of the CeO2 is 20-50nm.

3. A 4 series aluminum alloy according to claim 1, characterized in that: The specific surface area of ​​CeO2 is 40-70m 2 / g.

4. A method for preparing the 4-series aluminum alloy according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Weigh the raw materials according to the mass percentage of the components of the aluminum alloy; (2) Melting the weighed raw materials at 660-670°C, heating to 740-750°C, adding a refining agent under a nitrogen atmosphere, and refining for 30 minutes to obtain refined aluminum liquid; (3) placing the refined aluminum liquid in a mold, casting at a casting temperature of 680° C., a casting speed of 520 mm / min, and a cooling water quenching of 120 tons / h to obtain a cast rod; (4) The cast rod is subjected to T6 heat treatment to obtain a 4 series aluminum alloy.

5. The method for preparing the 4-series aluminum alloy according to claim 4, characterized in that: The refining agent is 65wt%Na2SiF6+35wt%C2Cl6.

6. The method for preparing the 4-series aluminum alloy according to claim 4, characterized in that: The amount of the refining agent added is 0.25% of the total mass of the raw materials.

7. The method for preparing the 4-series aluminum alloy according to claim 4, characterized in that: The T6 heat treatment specifically includes solution treatment at 500-510° C. for 2-4 hours; hot water quenching at 70-75° C. for 5-10 minutes; and aging treatment at 170-180° C. for 14-16 hours.

8. The method for preparing the 4-series aluminum alloy according to claim 7, characterized in that: The T6 heat treatment specifically includes solution treatment at 505° C. for 3 h, hot water quenching at 72° C. for 8 min, and aging treatment at 175° C. for 15 h.

9. Use of the 4 series aluminum alloy according to any one of claims 1 to 3.

10. Application of a 4-series aluminum alloy prepared according to the preparation method according to any one of claims 4 to 8.