Flame retardant antistatic fiber fabric and preparation method thereof
By grafting a flame retardant that reacts with cyanuric chloride and sodium sulfide with sepiolite, and combining it with nano-zinc oxide and water-based polyurethane, the problems of textile flammability and insufficient antistatic properties are solved, and a fabric with excellent flame retardancy is prepared. , fiber fabrics with antistatic and antibacterial properties.
Patent Information
- Application Number
- CN202410635354.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-22
AI Technical Summary
Existing textiles are flammable and have insufficient antistatic properties, which limits their application. In particular, polyester fabrics are prone to static electricity during processing, affecting comfort and softness.
The flame retardant obtained by the reaction of cyanuric chloride and sodium sulfide is grafted with sepiolite, and functionalized sepiolite is formed through amination and esterification treatment, and combined with nano zinc oxide and water-based polyurethane, through melt spinning and Preparation of flame retardant and antistatic fiber fabrics by impregnation treatment.
It significantly improves the flame retardancy, antistatic and antibacterial properties of fiber fabrics, forming a porous carbon layer to prevent heat transfer and oxygen diffusion, while enhancing the dispersion and compatibility of the fabric and improving the overall performance.
Smart Images

Figure CN118241487B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabrics, and in particular to a flame-retardant and antistatic fiber fabric and a preparation method thereof. Background Art
[0002] At present, most textiles are flammable. The softness and large surface area of textiles make them in contact with oxygen and heat in high temperature or flame environment, which makes them more likely to decompose and burn and spread rapidly. Polyester fabric is a widely used clothing fabric. Due to its poor hygroscopicity and low moisture regain, it is easy to generate static electricity during processing and wearing, causing many adverse effects. Therefore, how to improve the flame retardant and antistatic properties of polyester fabrics is an important research direction in the field of flame retardant materials research.
[0003] Existing technologies such as Chinese patent application CN104178879A disclose a radiation-proof flame-retardant fabric and a preparation method thereof, wherein mercerized cotton fiber is woven into a comfort layer with modal fiber and milk protein fiber, polyester and metal wire are blended into a radiation-proof flame-retardant layer, and polyester fiber, nano far-infrared ceramic fiber, bamboo charcoal fiber, corn fiber, chitin fiber and polyethylene fiber are blended into a radiation-proof flame-retardant layer, and the resulting fabric has flame-retardant and radiation-proof capabilities. However, the antibacterial properties and flame-retardant effects of the resulting fabric need to be improved, and the blending of metal wire and polyester fiber has insufficient comfort and softness, which limits the application of the fabric.
[0004] Prior art, such as Chinese patent application CN114434909A, discloses a highly flame-retardant and breathable protective fabric and a preparation method thereof, wherein a base fabric is formed by blending modified ramie fiber with polyester fiber, a flame-retardant layer is grafted onto one side of the base fabric, and the flame-retardant layer is modified on one side so that the contact surface between the flame-retardant layer and the base fabric has more active groups, which can react with the groups on the base fabric during the hot pressing process of the flame-retardant layer and the base fabric, thereby making the adhesion between them stronger; in addition, the flame retardant contains fluorine-containing side chains, and due to the low surface energy of the fluorine-containing side chains, the flame retardant layer is endowed with water resistance and chemical resistance, thereby improving the anti-fouling performance of the fabric, and at the same time, under the action of the migration of the fluorine-containing side chains, the cage-like phosphate structure in the flame retardant is more easily enriched on the surface of the composite material to form a dense protective carbon layer to prevent dripping or punching, thereby further improving the flame retardant performance of the flame retardant layer. However, the fabric produced by the method contains fluorine, which has excellent flame retardant properties as a halogen flame retardant, but releases harmful gases at high temperatures, which are harmful to human health and the environment. In addition, the antibacterial and antistatic properties of the fabric produced are insufficient, which limits the application of the fabric. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a flame retardant and antistatic fiber fabric and a preparation method thereof. The flame retardant and antistatic fiber fabric has excellent flame retardancy, antistatic properties and antibacterial properties.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a flame retardant antistatic fiber fabric comprises the following steps:
[0008] Step (1), mixing cyanuric chloride and acetone, adding sodium sulfide and hydrochloric acid aqueous solution, reacting, filtering, washing and drying after the reaction is completed to obtain a flame retardant;
[0009] Step (2), mixing sepiolite with a hydrochloric acid aqueous solution, reacting for the first time, filtering after the reaction is completed, washing, and obtaining hydroxylated sepiolite; mixing the hydroxylated sepiolite with water, ultrasonically dispersing, adding an ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the second time, centrifuging after the reaction is completed, filtering, taking a centrifugal precipitate, washing, and drying, and obtaining an amination sepiolite;
[0010] The aminated sepiolite, maleic anhydride and N,N-dimethylformamide are mixed and reacted for the first time. After the reaction is completed, the filter is sucked out, the filter cake is taken out, and the filter cake is washed to obtain the modified sepiolite; the modified sepiolite, flame retardant, sodium carbonate aqueous solution and phosphate buffer solution are mixed and reacted for the second time. After the reaction is completed, the filter is taken out, the filter cake is washed and dried to obtain the functionalized sepiolite;
[0011] Step (3), mixing the functionalized sepiolite with polyethylene terephthalate, melt spinning, cooling, drawing, and chopping to obtain modified polyester fiber; spinning the modified polyester fiber into yarn as warp and weft, weaving to obtain a surface fabric and a lining fabric, respectively;
[0012] The surface fabric and the inner fabric are laminated and aligned, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine using sewing thread to obtain a composite fabric;
[0013] Step (4), mixing nano zinc oxide with water, ultrasonically dispersing, adding ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the first time, centrifuging, filtering, taking the centrifugal precipitate, washing, and drying to obtain modified nano zinc oxide; mixing the modified nano zinc oxide with hydroxy silicone oil, reacting for the second time, and obtaining modified silicone oil after the reaction is completed;
[0014] Mix polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate and react; after the reaction is completed, add modified silicone oil and acetone and continue to react; after the reaction is completed, add triethylamine for neutralization to obtain modified waterborne polyurethane; mix the modified waterborne polyurethane with water and stir, stir evenly, and remove acetone by rotary evaporation to obtain a modified waterborne polyurethane finishing liquid;
[0015] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid, and after the impregnation, the composite fabric is baked and washed to obtain a flame retardant and antistatic fiber fabric.
[0016] Preferably, in step (1), the mass ratio of cyanuric chloride to acetone is 1:20-30; the mass ratio of cyanuric chloride, sodium sulfide and 1 mol / L hydrochloric acid aqueous solution is 20-25:15-18:30-50; and the reaction conditions are: reaction at a temperature of 0-5°C for 3-4h.
[0017] Furthermore, the hydrochloric acid aqueous solution is a 1 mol / L hydrochloric acid aqueous solution.
[0018] Preferably, in step (2), the mass ratio of sepiolite to aqueous hydrochloric acid solution is 1:20; and the first reaction conditions are: the first reaction is carried out at a temperature of 60-70° C. for 2-3 hours.
[0019] Furthermore, the hydrochloric acid aqueous solution is a 1 mol / L hydrochloric acid aqueous solution.
[0020] Preferably, in step (2), the mass ratio of hydroxylated sepiolite, ethanol aqueous solution and γ-aminopropyltriethoxysilane is 1:(90-100):10, and the ethanol aqueous solution is 50wt% ethanol aqueous solution; the second reaction conditions are: the second reaction is carried out at a temperature of 40-50°C for 10-18h;
[0021] Preferably, in step (2), the mass ratio of amination sepiolite, maleic anhydride and N,N-dimethylformamide is (8-10):(10-15):(80-100); and the first reaction conditions are: the first reaction is carried out at a temperature of 70-80° C. for 3-4 hours.
[0022] Preferably, in step (2), the mass ratio of modified sepiolite, flame retardant, sodium carbonate aqueous solution and phosphate buffer solution is (1-2):(5-10):(50-80):(300-500); the second reaction conditions are: the second reaction is carried out at a temperature of 40-50° C. for 12-18 hours.
[0023] Furthermore, the sodium carbonate aqueous solution is a 10 wt % sodium carbonate aqueous solution; and the phosphate buffer solution is a 0.1 mol / L phosphate buffer solution.
[0024] Preferably, in the step (3), the mass ratio of the functionalized sepiolite to the polyethylene terephthalate is (1-3):100; the melt spinning comprises: melt extrusion through a twin-screw melt spinning machine at a spinning speed of 1500-2000 m / min under the condition that the temperature of each zone of the extruder is 250-255°C; the fineness of the modified polyester fiber is 70D and the average length is 38 mm; the yarn spun from the modified polyester fiber is used as the warp and weft, and the English count of the yarn is 60S.
[0025] Preferably, the sewing thread comprises polyester sewing thread.
[0026] Preferably, in step (3): the weight of the surface layer fabric is 240-260 g / m 2 ; The weight of the inner layer fabric is 200-220g / m 2 ;
[0027] Preferably, in step (4), the mass ratio of nano zinc oxide, ethanol aqueous solution and γ-aminopropyltriethoxysilane is 1:(90-100):10, the ethanol aqueous solution is 50wt% ethanol aqueous solution; the first reaction conditions are: the first reaction is carried out at a temperature of 40-50°C for 10-18h; the mass ratio of modified nano zinc oxide to hydroxy silicone oil is 1:10; the second reaction conditions are: the second reaction is carried out at a temperature of 110-120°C for 5-6h.
[0028] Preferably, in step (4), the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone and triethylamine is (180-200):(100-120):(2-3):(25-50):(50-60):(25-30); the reaction conditions are: reacting at 70-80°C for 3-4h in a nitrogen atmosphere; continuing the reaction conditions are: continuing the reaction at 50-60°C for 4-5h; the neutralization conditions are: cooling to 30-40°C and neutralizing for 10-20min; and the solid content of the modified waterborne polyurethane finishing liquid is 38%.
[0029] Preferably, in step (4), the bath ratio of the composite fabric to the modified waterborne polyurethane finishing liquid is 1:300; the dipping operation comprises: dipping at room temperature for 20-30 minutes, one dipping and one rolling, and the rolling rate is 75%; the baking conditions are: pre-baking at 90-100°C for 1-2 minutes, and baking at 150-160°C for 2-3 minutes.
[0030] Preferably, a flame retardant antistatic fiber fabric is prepared by the method for preparing the flame retardant antistatic fiber fabric as described above.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] Triazine derivatives are flame retardant foaming agents. When a polymer with such flame retardants is heated and burned, a porous foamed carbon layer can be generated on the surface. The carbon layer can prevent the transfer of heat and the diffusion of oxygen in the condensed phase, reduce the release of combustible gas and smoke, and prevent the melting droplet behavior generated by the combustion of the polymer, which can well protect the polymer that is in long-term or repeated contact with the flame. In the present invention, cyanuric chloride is reacted with sodium sulfide, so that the flame retardant molecule obtained has a mercapto group. Among them, the mercapto group provides an active group for the grafting reaction between the flame retardant and sepiolite.
[0033] Sepiolite is a fibrous layered magnesium silicate clay mineral with low thermal conductivity, high temperature resistance, and non-halogen flame retardant elements such as magnesium and silicon. Therefore, it can be used as a flame retardant filler and composited with high molecular polymers to improve the flame retardant effect of the material. After the sepiolite is acidified, it is reacted with γ-aminopropyltriethoxysilane to obtain amination sepiolite, and the amination sepiolite is grafted with maleic anhydride, and then the double bond in the grafted maleic anhydride is subjected to Michael addition reaction with the thiol group of the flame retardant to graft the flame retardant on the amination sepiolite, which improves the dispersibility of sepiolite in the matrix and the stability of the flame retardant, making it difficult for the flame retardant to migrate, and making the obtained functionalized sepiolite have better flame retardant effect.
[0034] The functionalized sepiolite is grafted onto the chain segments of polyethylene terephthalate through an esterification reaction between the carboxyl groups on the surface of the functionalized sepiolite and the terminal hydroxyl groups of the polyethylene terephthalate molecular chains in the molten state. This makes the functionalized sepiolite have better dispersibility and compatibility in the polyethylene terephthalate, thereby improving the flame retardant properties and mechanical properties of the modified polyester.
[0035] Nano zinc oxide is a metal oxide with certain conductivity and excellent antibacterial properties. The modified nano zinc oxide obtained by reacting nano zinc oxide with γ-aminopropyltriethoxysilane has an amino group. The amino group of the modified nano zinc oxide reacts with the hydroxyl group of the hydroxy silicone oil to fix the modified nano zinc oxide in the chain segment of the hydroxy silicone oil, so that the modified nano zinc oxide is not easy to fall off. The modified silicone oil obtained has excellent antistatic and antibacterial properties; the modified silicone oil is used as a chain extender to extend the chain of the waterborne polyurethane prepolymer, and the modified waterborne polyurethane obtained is rich in hydrophilic groups and has excellent antistatic properties. At the same time, the siloxane segments in the modified silicone oil give the waterborne polyurethane excellent flame retardant effects, so the finishing liquid prepared by the modified waterborne polyurethane has flame retardant, antistatic and antibacterial properties. The flame retardant and antistatic fiber fabric obtained after padding the composite fabric also has excellent flame retardant, antistatic and antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a process flow chart for preparing flame-retardant and antistatic fiber fabrics in the present invention;
[0037] Figure 2 It is a schematic structural diagram of the flame-retardant and antistatic fiber fabric prepared in the present invention;
[0038] Figure 3 It is a histogram of the limiting oxygen index in the flame retardant performance test of the flame retardant antistatic fiber fabrics prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention;
[0039] Figure 4 It is a bar graph of the damaged length in the flame retardant performance test of the flame retardant antistatic fiber fabrics prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention;
[0040] Figure 5 It is a bar graph of the antibacterial rate in the antibacterial performance test of the flame-retardant and antistatic fiber fabrics prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention;
[0041] In the figure:
[0042] 1. Surface fabric; 2. Lining fabric. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1
[0044] This embodiment discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0045] Step (1), mixing cyanuric chloride and acetone in a mass ratio of 1:25, adding sodium sulfide and 1 mol / L hydrochloric acid aqueous solution, reacting at 2°C for 3 hours, filtering after the reaction to obtain a crude reaction product, adding water 6 times the mass of the crude reaction product for washing, and drying at 55°C for 10 hours to obtain a flame retardant;
[0046] The mass ratio of cyanuric chloride, sodium sulfide and 1 mol / L hydrochloric acid aqueous solution is 22:16:40;
[0047] Step (2), mixing sepiolite with 1 mol / L hydrochloric acid aqueous solution at a mass ratio of 1:20, reacting for the first time at 65°C for 2 hours, filtering and washing after the reaction to obtain hydroxylated sepiolite; mixing hydroxylated sepiolite with water at a mass ratio of 1:250, ultrasonically dispersing for 20 minutes, adding 50 wt% ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the second time at 45°C for 14 hours, centrifuging at 3500 r / min for 10 minutes, filtering, taking the centrifugal precipitate, adding ethanol 10 times the mass of the centrifugal precipitate to wash three times, and drying at 55°C for 20 hours to obtain amination sepiolite;
[0048] The mass ratio of hydroxylated sepiolite, 50 wt% ethanol aqueous solution, and γ-aminopropyltriethoxysilane is 1:90:10;
[0049] The aminated sepiolite, maleic anhydride and N,N-dimethylformamide were mixed in a mass ratio of 8:10:80, and the mixture was reacted for a first time at 70°C for 4 hours. After the reaction was completed, the filter cake was filtered and washed with ethanol 5 times the mass of the filter cake to obtain the modified sepiolite.
[0050] The modified sepiolite, the flame retardant, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 1:5:50:300, and the mixture was reacted for a second time at 50° C. for 12 h. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 5 times the mass of the filter cake was added for washing, and the mixture was dried at 50° C. for 12 h to obtain the functionalized sepiolite;
[0051] Step (3), mixing functionalized sepiolite and polyethylene terephthalate in a mass ratio of 3:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 250° C., spinning at a spinning speed of 1500 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0052] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0053] Among them, the weight of the surface fabric is 240g / m 2 ; The weight of the inner layer fabric is 220g / m 2 ;
[0054] Step (4), mixing nano zinc oxide with water at a mass ratio of 1:250, ultrasonically dispersing for 20 minutes, adding 50wt% ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the first time at 45°C for 15 hours, centrifuging at a speed of 3500r / min for 10 minutes after the reaction, filtering, taking the centrifugal precipitate, adding ethanol 6 times the mass of the centrifugal precipitate to wash three times, and drying at 55°C for 20 hours to obtain modified nano zinc oxide; mixing the modified nano zinc oxide with hydroxy silicone oil at a mass ratio of 1:10, reacting for the second time at 115°C for 5 hours, and obtaining modified silicone oil after the reaction;
[0055] The mass ratio of nano zinc oxide, 50 wt% ethanol aqueous solution, and γ-aminopropyltriethoxysilane is 1:100:10;
[0056] The polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate were mixed and reacted in a nitrogen atmosphere at 70°C for 4 hours; after the reaction, modified silicone oil and acetone were added and the reaction was continued at 50°C for 5 hours. After the reaction was completed, the temperature was lowered to 30°C, and triethylamine was added for neutralization for 20 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane was mixed and stirred with water at room temperature for 20 minutes. After stirring evenly, the acetone was removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid;
[0057] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid at room temperature for 30 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 90°C for 2 minutes, baked at 150°C for 3 minutes, and washed with water to obtain a flame-retardant antistatic fiber fabric.
[0058] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone and triethylamine is 180:100:3:50:60:25; the solid content of the modified water-based polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified water-based polyurethane finishing liquid is 1:300, and the roll-off rate of the impregnation operation is 75%. Example 2
[0059] This embodiment discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0060] Step (1), preparing a flame retardant;
[0061] The preparation steps of the flame retardant are the same as those in Example 1;
[0062] Step (2), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 10:15:100, reacting for a first time at 80° C. for 3 h, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount 8 times the mass of the filter cake to obtain a modified sepiolite;
[0063] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0064] The modified sepiolite, the flame retardant, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 2:10:80:500, and reacted for a second time at 40° C. for 18 h. After the reaction was completed, the filter cake was taken out, and water 8 times the mass of the filter cake was added for washing, and the filter cake was dried at 60° C. for 8 h to obtain the functionalized sepiolite;
[0065] Step (3), mixing functionalized sepiolite and polyethylene terephthalate in a mass ratio of 2.5:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 255° C., spinning at a spinning speed of 2000 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0066] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0067] Among them, the weight of the surface fabric is 260g / m 2 ; The weight of the inner layer fabric is 200g / m 2 ;
[0068] Step (4), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted at 80°C for 3 hours in a nitrogen atmosphere; after the reaction, modified silicone oil and acetone are added, and the mixture is reacted at 60°C for 4 hours; after the reaction, the mixture is cooled to 40°C, and triethylamine is added for neutralization for 10 minutes to obtain a modified waterborne polyurethane; the modified waterborne polyurethane is mixed and stirred with water at room temperature for 30 minutes, and after uniform stirring, the acetone is removed by rotary evaporation at 40°C to obtain a modified waterborne polyurethane finishing liquid;
[0069] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid at room temperature for 20 minutes, and the mixture is immersed and rolled. After the impregnation, the composite fabric is pre-baked at 100° C. for 1 minute, and then baked at 160° C. for 2 minutes, and then washed to obtain a flame-retardant antistatic fiber fabric.
[0070] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 185:105:3:40:60:25; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the rolling rate of the dipping operation is 75%;
[0071] The preparation steps of the modified silicone oil are the same as those in Example 1. Example 3
[0072] This embodiment discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0073] Step (1), preparing a flame retardant;
[0074] The preparation steps of the flame retardant are the same as those in Example 1;
[0075] Step (2), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 9:12:90, reacting for a first time at 75°C for 3.5 hours, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount of 6 times the mass of the filter cake to obtain a modified sepiolite;
[0076] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0077] The modified sepiolite, the flame retardant, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 1:8:60:400, and the mixture was reacted for a second time at 45° C. for 14 h. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 6 times the mass of the filter cake was added for washing, and the mixture was dried at 55° C. for 10 h to obtain the functionalized sepiolite;
[0078] Step (3), mixing functionalized sepiolite with polyethylene terephthalate in a mass ratio of 2:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 253° C., spinning at a spinning speed of 1800 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0079] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0080] Among them, the weight of the surface fabric is 250g / m 2; The weight of the inner layer fabric is 210g / m 2 ;
[0081] Step (4), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted in a nitrogen atmosphere at 75°C for 3.5 hours; after the reaction is completed, modified silicone oil and acetone are added, and the reaction is continued at 55°C for 4.5 hours. After the reaction is completed, the mixture is cooled to 35°C, and triethylamine is added for neutralization for 15 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane is mixed and stirred with water at room temperature for 25 minutes. After being uniformly stirred, the acetone is removed by rotary evaporation at 45°C to obtain a modified waterborne polyurethane finishing liquid;
[0082] The composite fabric is impregnated with the modified waterborne polyurethane finishing liquid at room temperature for 25 minutes, and the mixture is immersed and rolled. After the immersion, the composite fabric is pre-baked at 95°C for 1 minute, baked at 155°C for 3 minutes, and washed with water to obtain a flame retardant and antistatic fiber fabric.
[0083] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 190:110:2:35:55:28; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the rolling rate of the dipping operation is 75%;
[0084] The preparation steps of the modified silicone oil are the same as those in Example 1. Example 4
[0085] This embodiment discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0086] Step (1), preparing a flame retardant;
[0087] The preparation steps of the flame retardant are the same as those in Example 1;
[0088] Step (2), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 10:14:90, reacting for the first time at 70° C. for 3 h, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount 8 times the mass of the filter cake to obtain a modified sepiolite;
[0089] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0090] The modified sepiolite, the flame retardant, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 2:6:70:500, and the mixture was reacted for a second time at 50° C. for 12 h. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 6 times the mass of the filter cake was added for washing, and the mixture was dried at 55° C. for 10 h to obtain the functionalized sepiolite;
[0091] Step (3), mixing functionalized sepiolite with polyethylene terephthalate in a mass ratio of 1.5:100, melt-extruded through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 255° C., spinning at a spinning speed of 1800 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0092] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0093] Among them, the weight of the surface fabric is 240g / m 2 ; The weight of the inner layer fabric is 210g / m 2 ;
[0094] Step (4), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted at 70°C for 4 hours in a nitrogen atmosphere; after the reaction, modified silicone oil and acetone are added, and the mixture is reacted at 50°C for 5 hours. After the reaction, the mixture is cooled to 40°C, and triethylamine is added for neutralization for 15 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane is mixed and stirred with water at room temperature for 25 minutes. After uniform stirring, the acetone is removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid.
[0095] The composite fabric is impregnated with the modified waterborne polyurethane finishing liquid at room temperature for 30 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 100°C for 1 minute, baked at 155°C for 3 minutes, and washed to obtain a flame retardant and antistatic fiber fabric.
[0096] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 195:115:2:30:50:30; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the residual rate of the dipping operation is 75%;
[0097] The preparation steps of the modified silicone oil are the same as those in Example 1. Example 5
[0098] This embodiment discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0099] Step (1), preparing a flame retardant;
[0100] The preparation steps of the flame retardant are the same as those in Example 1;
[0101] Step (2), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 8:11:80, reacting for the first time at 80° C. for 3 h, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount of 8 times the mass of the filter cake to obtain a modified sepiolite;
[0102] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0103] The modified sepiolite, the functionalized cyclophosphazene, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 1:5:50:400, and the mixture was reacted for a second time at 40° C. for 18 h. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 8 times the mass of the filter cake was added for washing, and the mixture was dried at 50° C. for 12 h to obtain the functionalized sepiolite;
[0104] Step (3), mixing functionalized sepiolite with polyethylene terephthalate in a mass ratio of 1:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 250° C., spinning at a spinning speed of 1500 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0105] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0106] Among them, the weight of the surface fabric is 250g / m 2 ; The weight of the inner layer fabric is 220g / m 2 ;
[0107] Step (4), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted at 80°C for 3 hours in a nitrogen atmosphere; after the reaction, modified silicone oil and acetone are added, and the mixture is reacted at 60°C for 4 hours; after the reaction, the mixture is cooled to 30°C, and triethylamine is added for neutralization for 20 minutes to obtain a modified waterborne polyurethane; the modified waterborne polyurethane is mixed and stirred with water at room temperature for 30 minutes, and after uniform stirring, the acetone is removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid;
[0108] The composite fabric is impregnated with the modified waterborne polyurethane finishing liquid at room temperature for 20 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 90°C for 2 minutes, baked at 160°C for 2 minutes, and washed with water to obtain a flame retardant and antistatic fiber fabric.
[0109] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 200:120:2:25:50:30; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the rolling rate of the dipping operation is 75%;
[0110] The preparation steps of the modified silicone oil are the same as those in Example 1.
[0111] Comparative Example 1
[0112] This comparative example discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0113] Step (1), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 8:10:80, reacting for a first time at 70° C. for 4 hours, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount 5 times the mass of the filter cake to obtain a modified sepiolite;
[0114] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0115] Step (2), mixing modified sepiolite and polyethylene terephthalate in a mass ratio of 3:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 250° C., spinning at a spinning speed of 1500 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0116] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0117] Among them, the weight of the surface fabric is 240g / m 2 ; The weight of the inner layer fabric is 220g / m 2 ;
[0118] Step (3), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted at 70°C for 4 hours in a nitrogen atmosphere; after the reaction is completed, modified silicone oil and acetone are added, and the reaction is continued at 50°C for 5 hours. After the reaction is completed, the mixture is cooled to 30°C, and triethylamine is added for neutralization for 20 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane is mixed and stirred with water at room temperature for 20 minutes. After uniform stirring, the acetone is removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid;
[0119] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid at room temperature for 30 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 90°C for 2 minutes, baked at 150°C for 3 minutes, and washed with water to obtain a flame-retardant antistatic fiber fabric.
[0120] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 180:100:3:50:60:25; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the rolling rate of the dipping operation is 75%;
[0121] The preparation steps of the modified silicone oil are the same as those in Example 1.
[0122] Comparative Example 2
[0123] This comparative example discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0124] Step (1), preparing a flame retardant;
[0125] The preparation steps of the flame retardant are the same as those in Example 1;
[0126] Step (2), mixing sepiolite, flame retardant and polyethylene terephthalate in a mass ratio of 3:5:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 250° C., spinning at a spinning speed of 1500 m / min, cooling, drawing and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0127] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0128] Among them, the weight of the surface fabric is 240g / m 2 ; The weight of the inner layer fabric is 220g / m 2 ;
[0129] Step (3), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and the mixture is reacted at 70°C for 4 hours in a nitrogen atmosphere; after the reaction is completed, modified silicone oil and acetone are added, and the reaction is continued at 50°C for 5 hours. After the reaction is completed, the mixture is cooled to 30°C, and triethylamine is added for neutralization for 20 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane is mixed and stirred with water at room temperature for 20 minutes. After uniform stirring, the acetone is removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid;
[0130] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid at room temperature for 30 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 90°C for 2 minutes, baked at 150°C for 3 minutes, and washed with water to obtain a flame-retardant antistatic fiber fabric.
[0131] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone, and triethylamine is 180:100:3:50:60:25; the solid content of the modified waterborne polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified waterborne polyurethane finishing liquid is 1:300, and the rolling rate of the dipping operation is 75%;
[0132] The preparation steps of the modified silicone oil are the same as those in Example 1.
[0133] Comparative Example 3
[0134] This comparative example discloses a method for preparing a flame retardant and antistatic fiber fabric, comprising the following steps:
[0135] Step (1), preparing a flame retardant;
[0136] The preparation steps of the flame retardant are the same as those in Example 1;
[0137] Step (2), mixing aminated sepiolite, maleic anhydride and N,N-dimethylformamide in a mass ratio of 8:10:80, reacting for a first time at 70° C. for 4 h, and after the reaction is completed, filtering to obtain a filter cake, and washing with ethanol in an amount 5 times the mass of the filter cake to obtain a modified sepiolite;
[0138] Wherein, the preparation steps of amination sepiolite are the same as those in Example 1;
[0139] The modified sepiolite, the flame retardant, the 10 wt % sodium carbonate aqueous solution, and the 0.1 mol / L phosphate buffer solution were mixed in a mass ratio of 1:5:50:300, and the mixture was reacted for a second time at 50° C. for 12 h. After the reaction was completed, the mixture was filtered, the filter cake was taken, and water 5 times the mass of the filter cake was added for washing, and the mixture was dried at 50° C. for 12 h to obtain the functionalized sepiolite;
[0140] Step (3), mixing functionalized sepiolite and polyethylene terephthalate in a mass ratio of 3:100, melt extruding through a twin-screw melt spinning machine under the condition that the temperature of each zone of the extruder is 250° C., spinning at a spinning speed of 1500 m / min, cooling, drawing, and chopping to obtain modified polyester fibers with a fineness of 70D and an average length of 38 mm; spinning the modified polyester fibers into yarns as warp and weft, the yarn counts of which are both 60S in English, and weaving to obtain surface fabrics and lining fabrics respectively;
[0141] The surface fabric and the inner fabric are laminated and aligned, and polyester sewing thread is used as the sewing thread, and the surface fabric and the inner fabric are sewn together by a multi-layer fabric quilting machine to obtain a composite fabric;
[0142] Among them, the weight of the surface fabric is 240g / m 2 ; The weight of the inner layer fabric is 220g / m 2 ;
[0143] Step (4), polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate are mixed, and reacted in a nitrogen atmosphere at 70°C for 4 hours; after the reaction, 2,2-dihydroxymethylpropionic acid and acetone are added, and the reaction is continued at 50°C for 5 hours. After the reaction is completed, the temperature is lowered to 30°C, and triethylamine is added for neutralization for 20 minutes to obtain a modified waterborne polyurethane. The modified waterborne polyurethane, nano zinc oxide and water are mixed and stirred at room temperature for 20 minutes. After stirring evenly, the acetone is removed by rotary evaporation at 50°C to obtain a modified waterborne polyurethane finishing liquid;
[0144] The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid at room temperature for 30 minutes, and the mixture is dipped and rolled. After the impregnation, the composite fabric is pre-baked at 90°C for 2 minutes, baked at 150°C for 3 minutes, and washed with water to obtain a flame-retardant antistatic fiber fabric.
[0145] Among them, the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, 2,2-dihydroxymethylpropionic acid, acetone and triethylamine is 180:100:3:50:60:25; the mass ratio of modified water-based polyurethane and nano-zinc oxide is 100:0.1; the solid content of the modified water-based polyurethane finishing liquid is 38%; the bath ratio of the composite fabric and the modified water-based polyurethane finishing liquid is 1:300, and the roll-off rate of the impregnation operation is 75%.
[0146] In the above embodiments and comparative examples:
[0147] Cyanuric chloride was from Shandong Poly Chemical Co., Ltd., CAS No.: 108-77-0; acetone was from Shandong Wenshao Chemical Co., Ltd., CAS No.: 67-64-1; sodium sulfide was from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS No.: 1313-82-2; hydrochloric acid aqueous solution was from Shanghai Yuanye Biotechnology Co., Ltd., item No. B62243, model hydrogen chloride standard solution; sepiolite was from Hebei Mingzhe Mineral Products Co., Ltd., density 2.3g / cm 3, fibrous in shape, particle size 120 mesh; hydrochloric acid aqueous solution comes from Shanghai Yuanye Biotechnology Co., Ltd., item number B62243, model hydrogen chloride standard solution; γ-aminopropyltriethoxysilane comes from Guangdong Lvwei New Materials Technology Co., Ltd., CAS number: 919-30-2; maleic anhydride comes from Wuxi Jingke Chemical Co., Ltd., CAS number: 108-31-6; N,N-dimethylformamide comes from Jinan Yuanxiang Chemical Co., Ltd., CAS number: 68-12-2; sodium carbonate comes from Wuxi Jingke Chemical Co., Ltd., CAS number: 497-19-8; phosphate buffer solution comes from Isejiu Biotechnology Co., Ltd., name PBS phosphate buffer; polyethylene terephthalate comes from Yanshan Petrochemical Company, model 63-SD, CAS number: 25038-59-9; polyester sewing thread comes from Yiwu Yingming Thread Co., Ltd., yarn count is 20S ( English count); Nano zinc oxide comes from Hangzhou Jikang New Materials Co., Ltd., product number SS-Z50, particle size 40-50nm, CAS number: 1314-13-2; hydroxy silicone oil comes from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., product name double-terminal hydroxyl-terminated polydimethylsiloxane, viscosity 800cs; polypropylene glycol comes from Guangzhou Jiangshun Chemical Technology Co., Ltd., molecular weight 2000, CAS number: 25322-69-4; 2,4-toluene diisocyanate comes from Wuhan Kanos Technology Co., Ltd., CAS number: 584-84-9; dibutyltin dilaurate comes from Maoming Xiongda Chemical Co., Ltd., CAS number: 77-58-7; triethylamine comes from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS number: 121-44-8; 2,2-dihydroxymethylpropionic acid comes from Hubei Wei's Chemical Reagent Co., Ltd., CAS number: 4767-03-7.
[0148] Test example
[0149] (1) Flame retardant performance test
[0150] The flame retardant antistatic fiber fabrics prepared in Examples 1-5 and Comparative Examples 1-3 were tested for flame retardant properties. The specific test results are shown in Table 1:
[0151] Table 1
[0152] Limiting oxygen index (%) Damaged length (mm) Example 1 32.5 125.2 Example 2 32.3 125.6 Example 3 32.2 125.6 Example 4 32.2 125.7 Example 5 32.1 125.9 Comparative Example 1 28.6 141.3 Comparative Example 2 30.8 133.1 Comparative Example 3 29.9 129.5
[0153] The testing of each index in Table 1 is based on the following standards: the limiting oxygen index is measured by GB / T5454-1997 "Textile Combustion Performance Test-Oxygen Index Method"; the damaged length is measured by GB / T 5455-1997 "Textile Combustion Energy Test-Vertical Method"; the flame retardant grade is measured by GB17591-2006 "Flame Retardant Fabrics".
[0154] It can be seen from the test results in Table 1 that the flame retardant and antistatic fiber fabric prepared by the present invention has excellent flame retardant properties.
[0155] In the present invention, cyanuric chloride is reacted with sodium sulfide, and the flame retardant molecules obtained have mercapto groups, wherein the mercapto groups provide active groups for the grafting reaction between the flame retardant and sepiolite.
[0156] Sepiolite is a fibrous layered magnesium silicate clay mineral with low thermal conductivity, high temperature resistance, and non-halogen flame retardant elements such as magnesium and silicon. Therefore, it can be used as a flame retardant filler and composited with high molecular polymers to improve the flame retardant effect of the material. After the sepiolite is acidified, it is reacted with γ-aminopropyltriethoxysilane to obtain amination sepiolite, and the amination sepiolite is grafted with maleic anhydride, and then the double bond in the grafted maleic anhydride is subjected to Michael addition reaction with the thiol group of the flame retardant to graft the flame retardant on the amination sepiolite, which improves the dispersibility of sepiolite in the matrix and the stability of the flame retardant, making it difficult for the flame retardant to migrate, and making the obtained functionalized sepiolite have better flame retardant effect. The functionalized sepiolite is grafted onto the chain segments of polyethylene terephthalate through an esterification reaction between the carboxyl groups on the surface of the functionalized sepiolite and the terminal hydroxyl groups of the polyethylene terephthalate molecular chain in a molten state. This makes the functionalized sepiolite have better dispersibility and compatibility in polyethylene terephthalate, thereby improving the flame retardant properties of the modified polyester.
[0157] In addition, the modified silicone oil in the modified waterborne polyurethane has a siloxane segment, which gives the waterborne polyurethane an excellent flame retardant effect. The finishing liquid prepared by the modified waterborne polyurethane is used to immerse the composite fabric in the padding treatment, which can further improve the flame retardant properties of the flame retardant antistatic fiber fabric.
[0158] In Comparative Example 1, only modified sepiolite was added without adding flame retardant. The modified sepiolite was used as a matrix without grafting cyanuric chloride derivatives with excellent flame retardancy. After the modified sepiolite was mixed with polyethylene terephthalate for melt spinning, the flame retardancy of the modified polyester obtained was reduced. Although the flame retardancy of the composite fabric was improved after padding with modified waterborne polyurethane, the flame retardancy of the comparative example 1 finally obtained was still lower than that of the embodiment.
[0159] In Comparative Example 2, the sepiolite was not surface modified and could not be grafted with the flame retardant through the Michael addition reaction. After adding it and the flame retardant to polyethylene terephthalate, the sepiolite had poor dispersibility and was easy to agglomerate. It could not undergo an esterification reaction with the terminal hydroxyl groups of the main chain of polyethylene terephthalate in the molten state to be fixed in the matrix resin. At the same time, the flame retardant was easy to migrate in polyethylene terephthalate, so the flame retardancy of the modified polyester was reduced. Although the flame retardancy of the composite fabric was improved after padding with the modified waterborne polyurethane, the flame retardancy of the final comparative example 2 was still lower than that of the embodiment.
[0160] In Comparative Example 3, no modified silicone oil is added to the modified water-based polyurethane finishing liquid, and the modified water-based polyurethane does not have a siloxane segment, so the flame retardant performance of the finishing liquid is reduced; although the composite fabric made of the modified polyester fiber has flame retardancy, after the composite fabric is impregnated with the modified water-based polyurethane finishing liquid, the flame retardancy of the final Comparative Example 3 is still lower than that of the embodiment.
[0161] (2) Antibacterial and antistatic properties test
[0162] The flame retardant antistatic fiber fabrics prepared in Examples 1-5 and Comparative Examples 1-3 were tested for antibacterial and antistatic properties. The specific test results are shown in Table 2:
[0163] Table 2
[0164]
[0165] The testing of each index in Table 2 is based on the following standards: the antibacterial rate is measured by GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", in which Escherichia coli is selected as the bacteria; the surface resistance is measured by GB / T22042-2008 "Test method for surface resistivity of antistatic properties of clothing".
[0166] It can be seen from the test results in Table 2 that the flame retardant antistatic fiber fabric prepared by the present invention has excellent antibacterial and antistatic properties.
[0167] Nano zinc oxide is a metal oxide with certain conductivity and excellent antibacterial properties. The modified nano zinc oxide obtained by reacting nano zinc oxide with γ-aminopropyltriethoxysilane has amino groups. The amino groups of the modified nano zinc oxide react with the hydroxyl groups of hydroxy silicone oil to fix the modified nano zinc oxide in the chain segments of hydroxy silicone oil, making it difficult for the modified nano zinc oxide to fall off. The modified silicone oil is used as a chain extender to extend the chain of waterborne polyurethane prepolymer. The modified waterborne polyurethane obtained is rich in hydrophilic groups and has excellent antistatic properties. Therefore, the finishing liquid prepared by the modified waterborne polyurethane has antistatic and antibacterial properties. The flame-retardant antistatic fiber fabric obtained after padding the composite fabric also has excellent antistatic and antibacterial properties.
[0168] In Comparative Example 3, no modified silicone oil is added to the modified water-based polyurethane finishing liquid, and the nano-zinc oxide is not polymerized with the polyurethane main chain. The nano-zinc oxide in the obtained modified water-based polyurethane is easy to agglomerate, so the antistatic and antibacterial properties of the finishing liquid are reduced; after the composite fabric is impregnated with the modified water-based polyurethane finishing liquid, the antistatic and antibacterial properties of the comparative example 3 finally obtained are lower than those in the embodiment.
[0169] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a flame retardant and antistatic fiber fabric, characterized in that: The following steps are involved: Step (1), mixing cyanuric chloride and acetone, adding sodium sulfide and hydrochloric acid aqueous solution, reacting, filtering, washing and drying after the reaction is completed to obtain a flame retardant; Step (2), mixing sepiolite with a hydrochloric acid aqueous solution, reacting for the first time, filtering after the reaction is completed, washing, and obtaining hydroxylated sepiolite; mixing the hydroxylated sepiolite with water, ultrasonically dispersing, adding an ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the second time, centrifuging after the reaction is completed, filtering, taking a centrifugal precipitate, washing, and drying, and obtaining an amination sepiolite; The aminated sepiolite, maleic anhydride and N,N-dimethylformamide are mixed and reacted for the first time. After the reaction is completed, the filter is filtered and the filter cake is taken and washed to obtain the modified sepiolite; The modified sepiolite, the flame retardant, the sodium carbonate aqueous solution and the phosphate buffer solution are mixed, reacted for the second time, filtered after the reaction is completed, the filter cake is taken, washed and dried to obtain the functionalized sepiolite; Step (3), mixing the functionalized sepiolite with polyethylene terephthalate, melt spinning, cooling, drawing, and chopping to obtain modified polyester fibers; The modified polyester fiber is spun into yarn as warp and weft, and woven to obtain the surface fabric and the inner fabric respectively; Compounding the surface layer fabric with the inner layer fabric to obtain a composite fabric; Step (4), mixing nano zinc oxide with water, ultrasonically dispersing, adding ethanol aqueous solution and γ-aminopropyltriethoxysilane, reacting for the first time, centrifuging, filtering, taking the centrifugal precipitate, washing, and drying to obtain modified nano zinc oxide; The modified nano zinc oxide is mixed with hydroxy silicone oil for a second reaction, and after the reaction is completed, the modified silicone oil is obtained; Mix polypropylene glycol, 2,4-toluene diisocyanate and dibutyltin dilaurate and react; after the reaction is completed, add modified silicone oil and acetone and continue to react; after the reaction is completed, add triethylamine for neutralization to obtain modified waterborne polyurethane; mix the modified waterborne polyurethane with water and stir, stir evenly, and remove acetone by rotary evaporation to obtain a modified waterborne polyurethane finishing liquid; The composite fabric is impregnated with a modified waterborne polyurethane finishing liquid, and after the impregnation, the composite fabric is baked and washed to obtain a flame retardant and antistatic fiber fabric; In the step (2), the mass ratio of sepiolite to hydrochloric acid aqueous solution is 1:20; the first reaction conditions are: the first reaction is carried out at a temperature of 60-70°C for 2-3 hours; the mass ratio of hydroxylated sepiolite, ethanol aqueous solution and γ-aminopropyltriethoxysilane is 1:(90-100):10, and the ethanol aqueous solution is a 50wt% ethanol aqueous solution; the second reaction conditions are: the second reaction is carried out at a temperature of 40-50°C for 10-18 hours; In the step (2), the mass ratio of amination sepiolite, maleic anhydride and N,N-dimethylformamide is (8-10):(10-15):(80-100); the first reaction conditions are: the first reaction is carried out at a temperature of 70-80° C. for 3-4 hours; In the step (4), the mass ratio of nano zinc oxide, ethanol aqueous solution and γ-aminopropyltriethoxysilane is 1:(90-100):10, and the ethanol aqueous solution is 50wt% ethanol aqueous solution; the first reaction condition is: the first reaction is carried out at a temperature of 40-50°C for 10-18h; the mass ratio of modified nano zinc oxide to hydroxy silicone oil is 1:10; the second reaction condition is: the second reaction is carried out at a temperature of 110-120°C for 5-6h.
2. The method for preparing a flame retardant and antistatic fiber fabric according to claim 1, characterized in that: In the step (1), the mass ratio of cyanuric chloride to acetone is 1:20-30; the mass ratio of cyanuric chloride, sodium sulfide and 1 mol / L hydrochloric acid aqueous solution is 20-25:15-18:30-50; and the reaction conditions are: reacting at a temperature of 0-5°C for 3-4h.
3. The method for preparing a flame retardant and antistatic fiber fabric according to claim 1, characterized in that: In the step (2), the mass ratio of modified sepiolite, flame retardant, sodium carbonate aqueous solution and phosphate buffer solution is (1-2):(5-10):(50-80):(300-500); the second reaction conditions are: the second reaction is carried out at a temperature of 40-50° C. for 12-18 hours.
4. The method for preparing a flame retardant and antistatic fiber fabric according to claim 1, characterized in that: In the step (3), the mass ratio of functionalized sepiolite to polyethylene terephthalate is (1-3):100; melt spinning comprises: melt extrusion through a twin-screw melt spinning machine at a spinning speed of 1500-2000 m / min under the condition that the temperature of each zone of the extruder is 250-255°C; the fineness of the modified polyester fiber is 70D and the average length is 38 mm; the yarn spun from the modified polyester fiber is used as the warp and weft, and the English count of the yarn is 60S; the gram weight of the surface fabric is 240-260 g / m 2 ; The weight of the inner layer fabric is 200-220g / m 2 .
5. The method for preparing a flame retardant and antistatic fiber fabric according to claim 1, characterized in that: In the step (4), the mass ratio of polypropylene glycol, 2,4-toluene diisocyanate, dibutyltin dilaurate, modified silicone oil, acetone and triethylamine is (180-200):(100-120):(2-3):(25-50):(50-60):(25-30); the reaction conditions are: reacting at 70-80°C for 3-4h in a nitrogen atmosphere; continuing the reaction conditions are: continuing the reaction at 50-60°C for 4-5h; the neutralization conditions are: cooling to 30-40°C and neutralizing for 10-20min; the solid content of the modified waterborne polyurethane finishing liquid is 38%.
6. The method for preparing a flame retardant and antistatic fiber fabric according to claim 1, characterized in that: In the step (4), the bath ratio of the composite fabric to the modified waterborne polyurethane finishing liquid is 1:300; the dipping operation includes: dipping at room temperature for 20-30 minutes, one dipping and one rolling, and the rolling rate is 75%; the baking conditions are: pre-baking at 90-100°C for 1-2 minutes, and baking at 150-160°C for 2-3 minutes.
7. A flame-retardant antistatic fiber fabric prepared by the method for preparing a flame-retardant antistatic fiber fabric as described in any one of claims 1 to 6.