Flame-retardant wear-resistant protective film and preparation method thereof
By using flame retardant polyurethane emulsion, graphene oxide modified ammonium polyphosphate and dopamine modified boron nitride in polymer membranes, the problem of insufficient flame retardant and wear resistance in traditional membranes is solved, and the fire is achieved High temperature stable flame retardant and wear-resistant effect in the case.
Patent Information
- Application Number
- CN202411435519.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polymer membranes have shortcomings in flame retardant and wear resistance, especially in fire situations, which are not well protected, making it difficult to meet the complex use environment and safety requirements of modern industrial and daily necessities.
Using a protective film consisting of flame-retardant polyurethane emulsion, auxiliary flame-retardant components and wear-resistant modified components, the combination of materials such as ammonium polyphosphate modification, and dopamine-modified boron nitride, etc., Protective films with excellent flame retardant and wear resistance were prepared.
It achieves stable flame retardant and wear resistance improvements at high temperatures, can effectively resist fire and wear, and significantly improve the service life and safety of the product.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer films, and in particular to a flame retardant and wear resistant protective film and a preparation method thereof. Background Art
[0002] In modern industry and daily life, surface protection is particularly important in the production and application of daily necessities such as shoes, leather goods, packaging and carpets. During use, these products need to have not only good aesthetics and durability, but also flame retardancy and wear resistance to cope with various complex use environments and potential safety risks. However, traditional protective films often fail to meet these requirements in terms of flame retardancy and wear resistance, especially in extreme situations such as fire, where the protective effect is greatly reduced.
[0003] In the current market, protective films for products such as shoes, leather goods, packaging and carpets are mostly made of materials such as polyolefins or polyesters. Although these materials can protect the surface of the product from scratches and pollution to a certain extent, they have obvious deficiencies in flame retardancy and wear resistance. Specifically, these protective films are easy to burn when exposed to fire, and have limited wear resistance, and cannot keep the product in good condition for a long time. Polyurethane, as a high-performance synthetic material, has excellent wear resistance, tear resistance, oil resistance and chemical resistance. At the same time, polyurethane materials can also introduce flame retardant groups through modification technology, thereby giving them flame retardant properties. Therefore, the development of a polyurethane protective film that has both excellent wear resistance and excellent flame retardant properties has become a problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a flame retardant and wear-resistant protective film and a preparation method thereof, which can effectively solve the problem of poor flame retardancy and wear resistance of the polymer film in the prior art.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A flame retardant and wear-resistant protective film, the flame retardant and wear-resistant protective film is composed of the following components: flame retardant polyurethane emulsion, auxiliary flame retardant component, wear-resistant modified component and silane coupling agent KH-560; The flame retardant polyurethane emulsion is prepared using phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dimethylol propionic acid as raw materials; The auxiliary flame retardant component is prepared by modifying ammonium polyphosphate with graphene oxide; The wear-resistant modified component is prepared by using dopamine-modified boron nitride and tetraethyl orthosilicate as raw materials.
[0006] Furthermore, the preparation method of the flame retardant polyurethane emulsion is: S2.1. Weigh 5-6g of phosphorus-containing polyol, 19-20g of polypropylene glycol, 15-16g of toluene diisocyanate and 3-4g of 2,2-dimethylol propionic acid into a flask, react at 85°C for 2h under nitrogen protection, dropwise add 8g of N'N-bis(2-hydroxymethyl)aminoethylphosphonic acid dimethyl ester and then add 20mL of butanone, continue to react for 2h, add 2-3g of triethylamine and react again for 10min, the obtained product is recorded as the prepolymer component; S2.2. Pour the prepolymer and 40-50 mL of deionized water into a high-speed shearing machine for high-speed shearing. After removing butanone by rotary evaporation, the resulting flame-retardant polyurethane emulsion is obtained.
[0007] Furthermore, the dripping rate in S2.1 is 1 drop / s, the specific operation of high-speed shearing in S2.2 is shearing at a rotation speed of 1000 r / min for 3-5 min, and the temperature of the rotary evaporation in S2.2 is 65°C.
[0008] Furthermore, the preparation method of the auxiliary flame retardant component is: S4.1. Weigh 7 g of ammonium polyphosphate and 0.5 g of silane coupling agent KH-550 and disperse them in 100 mL of anhydrous ethanol. Stir and react for 5 h in a water bath at 100 °C. The result is recorded as the reaction system. Weigh 1 g of graphene oxide and disperse it in 1 L of deionized water. After ultrasonic dispersion, it is recorded as the graphene oxide dispersion. S4.2. Add 20 mL of graphene oxide dispersion into the reaction system, then place it in a water bath at 100°C and stir the reaction for 5 hours. Wash the solid product with deionized water 5 times and then freeze-dry it to obtain the auxiliary flame retardant component.
[0009] Furthermore, the stirring speed of the stirring reaction in S4.1 is 300 r / min, the specific operation of ultrasonic dispersion in S4.1 is ultrasonic dispersion at a frequency of 28 kHz for 10 min, and the stirring speed of the stirring reaction in S4.2 is 400 r / min.
[0010] Furthermore, the preparation method of the wear-resistant modified component is: S6.1. Weigh 3 g of boron nitride and disperse it in 1 L of isopropanol. After ultrasonic oscillation, perform the first centrifugation. Take the upper suspension and perform the second centrifugation. The obtained supernatant is naturally air-dried and recorded as pretreated boron nitride. S6.2, weigh 3g of pretreated boron nitride and disperse it in 400mL of deionized water, add 0.5g of dopamine hydrochloride after ultrasonic oscillation, add tris(hydroxymethyl)aminomethane dropwise under stirring to adjust the pH value to 7.8, and finally react at 70°C for 5h, and filter to obtain dopamine-modified boron nitride; S6.3. Weigh 3 g of dopamine-modified boron nitride and disperse it in 300 mL of deionized water. Add tris(hydroxymethyl)aminomethane) to adjust the pH value to 8, then add 3 mL of tetraethyl orthosilicate. Stir the reaction for 6 hours and then age it for 2 hours. Then add 0.3 g of silane coupling agent KH-570 and continue stirring the reaction for 3 hours. After filtering, the precipitate is washed 3 times with deionized water and 3 times with ethanol to obtain the wear-resistant modified component.
[0011] Furthermore, in S6.1, the specific operation of ultrasonic oscillation is ultrasonic oscillation at a power of 200 W for 24 hours, the specific operation of the first centrifugation is centrifugation at a speed of 4000 r / min for 10 minutes, and the specific operation of the second centrifugation is centrifugation at a speed of 8000 r / min for 10 minutes.
[0012] Furthermore, in S6.2, the specific operation of ultrasonic oscillation is ultrasonic oscillation at a power of 200 W for 5 hours, the stirring speed of the stirring conditions is 300 r / min, and the dripping rate is 1 drop / s. In S6.3, the stirring speed of the stirring reaction is 200 r / min, and the dripping rate is 1 drop / s.
[0013] A method for preparing a flame retardant and wear-resistant protective film, the preparation method comprising: S1. Weigh 100 parts of flame-retardant polyurethane emulsion, 5-6 parts of auxiliary flame-retardant component, 8-10 parts of wear-resistant modification component and 1-2 parts of silane coupling agent KH-560 according to weight, mix them, and record them as emulsion components after mixing and dispersing them evenly; S2. Pour the emulsion components into a polytetrafluoroethylene mold, and after drying, obtain a flame retardant and wear-resistant protective film.
[0014] Furthermore, the specific operation of uniform mixing and dispersion in S1 is stirring at a stirring speed of 200 r / min for 30 minutes, and the specific operation of drying in S2 is first drying at room temperature for 7 days, and then drying in a vacuum drying oven at 60° C. for 4 hours.
[0015] The present invention provides a flame retardant and wear resistant protective film and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dihydroxymethyl propionic acid as raw materials to prepare a flame-retardant polyurethane emulsion. The flame-retardant polyurethane emulsion is a phosphorus-containing polyurethane co-modified with soft and hard segments. The phosphorus-containing polyol is used as a chain extender to introduce a stable flame-retardant molecular segment into the molecular chain of the polyurethane, so that the prepared flame-retardant polyurethane emulsion has stable flame-retardant properties. Secondly, the present invention modifies ammonium polyphosphate with graphene oxide to obtain an auxiliary flame-retardant component. Adding the auxiliary flame-retardant component to the flame-retardant polyurethane emulsion can improve the compatibility of ammonium polyphosphate with polyurethane, and make ammonium polyphosphate and phosphorus-containing polyol work together to further enhance the flame-retardant properties of the polyurethane emulsion. Graphene oxide can form a carbon layer at high temperature to prevent the transfer of heat and oxygen. Therefore, the addition of graphene oxide can improve the thermal stability and flame-retardant properties of the polyurethane emulsion. 2. The present invention deposits silicon dioxide on the surface of dopamine-modified boron nitride to obtain a wear-resistant modified component, which is added to a flame-retardant polyurethane emulsion to prepare a protective film, which can improve the wear resistance of the protective film; through the modification of dopamine, abundant hydroxyl functional groups can be introduced on the surface of boron nitride, thereby enhancing the bonding ability between boron nitride and silicon dioxide, and silicon dioxide, as an inorganic nanomaterial, has excellent hardness and wear resistance. After being deposited on the surface of dopamine-modified boron nitride, it can form a strong and wear-resistant protective layer, so that the protective film can effectively resist damage when it is subjected to friction or wear, thereby improving the wear resistance of the protective film. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] The present invention will be further described below in conjunction with the embodiments.
[0018] Example 1
[0019] A flame retardant and wear-resistant protective film of this embodiment, the flame retardant and wear-resistant protective film is composed of the following components: flame retardant polyurethane emulsion, auxiliary flame retardant component, wear-resistant modified component and silane coupling agent KH-560; The flame retardant polyurethane emulsion is prepared from phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dimethylol propionic acid as raw materials, wherein the preparation method of the flame retardant polyurethane emulsion is as follows: S2.1. Weigh 5 g of phosphorus-containing polyol, 19 g of polypropylene glycol, 15 g of toluene diisocyanate and 3 g of 2,2-dimethylol propionic acid into a flask, react at 85°C for 2 h under nitrogen protection, then add 8 g of N'N-bis(2-hydroxymethyl)aminoethylphosphonic acid dimethyl ester at a rate of 1 drop / s, then add 20 mL of butanone, continue to react for 2 h, then add 2 g of triethylamine and react again for 10 min. The result is recorded as the prepolymer component; S2.2. Pour the prepolymer and 40 mL of deionized water into a high-speed shearing machine and shear at a speed of 1000 r / min for 3 minutes. After removing butanone by rotary evaporation at a temperature of 65°C, the resulting flame-retardant polyurethane emulsion is obtained.
[0020] The auxiliary flame retardant component is prepared by modifying ammonium polyphosphate with graphene oxide, wherein the preparation method of the auxiliary flame retardant component is: S4.1. Weigh 7 g of ammonium polyphosphate and 0.5 g of silane coupling agent KH-550 and disperse them in 100 mL of anhydrous ethanol. Stir the mixture in a water bath at 100 °C at a stirring speed of 300 r / min for 5 h. The result is recorded as the reaction system. Weigh 1 g of graphene oxide and disperse it in 1 L of deionized water. Ultrasonic dispersion is performed at a frequency of 28 kHz for 10 min and recorded as the graphene oxide dispersion. S4.2. Add 20 mL of graphene oxide dispersion into the reaction system, and then place it in a water bath at 100°C and stir at a speed of 400 r / min for 5 hours. Wash the solid product with deionized water 5 times and then freeze-dry it to obtain the auxiliary flame retardant component.
[0021] The wear-resistant modified component is prepared by using dopamine-modified boron nitride and tetraethyl orthosilicate as raw materials, wherein the preparation method of the wear-resistant modified component is as follows: S6.1. Weigh 3 g of boron nitride and disperse it in 1 L of isopropanol. Ultrasonicate at 200 W for 24 h and centrifuge at 4000 r / min for 10 min. Take the upper suspension and centrifuge at 8000 r / min for 10 min. The supernatant is naturally air-dried and recorded as pretreated boron nitride. S6.2, weigh 3g of pretreated boron nitride and disperse it in 400mL of deionized water, add 0.5g of dopamine hydrochloride after ultrasonic oscillation at a power of 200W for 5h, add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s under stirring at a speed of 300r / min to adjust the pH value to 7.8, and finally react at a temperature of 70°C for 5h, and filter to obtain dopamine-modified boron nitride; S6.3. Weigh 3 g of dopamine-modified boron nitride and disperse it in 300 mL of deionized water. Add tris(hydroxymethyl)aminomethane at a drop rate of 1 drop / s to adjust the pH value to 8, then add 3 mL of tetraethyl orthosilicate. Stir the mixture at a stirring speed of 200 r / min for 6 hours and then age it for 2 hours. Then add 0.3 g of silane coupling agent KH-570 and continue stirring the reaction for 3 hours. After filtering, the precipitate is washed 3 times with deionized water and 3 times with ethanol in turn to obtain the wear-resistant modified component.
[0022] A method for preparing a flame retardant and wear-resistant protective film, the preparation method comprising: S1. Weigh 100 parts of flame-retardant polyurethane emulsion, 5 parts of auxiliary flame-retardant component, 8 parts of wear-resistant modified component and 1 part of silane coupling agent KH-560 according to weight, mix them, stir at a stirring speed of 200 r / min for 30 minutes, and record them as emulsion components; S2. Pour the emulsion components into a polytetrafluoroethylene mold, dry it at room temperature for 7 days, and then dry it in a vacuum drying oven at 60°C for 4 hours to obtain a flame retardant and wear-resistant protective film.
[0023] Example 2
[0024] A flame retardant and wear-resistant protective film of this embodiment, the flame retardant and wear-resistant protective film is composed of the following components: flame retardant polyurethane emulsion, auxiliary flame retardant component, wear-resistant modified component and silane coupling agent KH-560; The flame retardant polyurethane emulsion is prepared from phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dimethylol propionic acid as raw materials, wherein the preparation method of the flame retardant polyurethane emulsion is as follows: S2.1. Weigh 6 g of phosphorus-containing polyol, 20 g of polypropylene glycol, 16 g of toluene diisocyanate and 4 g of 2,2-dimethylol propionic acid into a flask, react at 85°C for 2 h under nitrogen protection, then add 8 g of N'N-bis(2-hydroxymethyl)aminoethylphosphonic acid dimethyl ester at a rate of 1 drop / s, then add 20 mL of butanone, continue to react for 2 h, then add 3 g of triethylamine and react again for 10 min. The result is recorded as the prepolymer component. S2.2. Pour the prepolymer and 50 mL of deionized water into a high-speed shearing machine and shear at a speed of 1000 r / min for 5 minutes. After removing butanone by rotary evaporation at a temperature of 65°C, the resulting flame-retardant polyurethane emulsion is obtained.
[0025] The auxiliary flame retardant component is prepared by modifying ammonium polyphosphate with graphene oxide, wherein the preparation method of the auxiliary flame retardant component is: S4.1. Weigh 7 g of ammonium polyphosphate and 0.5 g of silane coupling agent KH-550 and disperse them in 100 mL of anhydrous ethanol. Stir the mixture in a water bath at 100 °C at a stirring speed of 300 r / min for 5 h. The result is recorded as the reaction system. Weigh 1 g of graphene oxide and disperse it in 1 L of deionized water. Ultrasonic dispersion is performed at a frequency of 28 kHz for 10 min and recorded as the graphene oxide dispersion. S4.2. Add 20 mL of graphene oxide dispersion into the reaction system, and then place it in a water bath at 100°C and stir at a speed of 400 r / min for 5 hours. Wash the solid product with deionized water 5 times and then freeze-dry it to obtain the auxiliary flame retardant component.
[0026] The wear-resistant modified component is prepared by using dopamine-modified boron nitride and tetraethyl orthosilicate as raw materials, wherein the preparation method of the wear-resistant modified component is as follows: S6.1. Weigh 3 g of boron nitride and disperse it in 1 L of isopropanol. Ultrasonicate at 200 W for 24 h and centrifuge at 4000 r / min for 10 min. Take the upper suspension and centrifuge at 8000 r / min for 10 min. The supernatant is naturally air-dried and recorded as pretreated boron nitride. S6.2, weigh 3g of pretreated boron nitride and disperse it in 400mL of deionized water, add 0.5g of dopamine hydrochloride after ultrasonic oscillation at a power of 200W for 5h, add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s under stirring at a speed of 300r / min to adjust the pH value to 7.8, and finally react at a temperature of 70°C for 5h, and filter to obtain dopamine-modified boron nitride; S6.3. Weigh 3 g of dopamine-modified boron nitride and disperse it in 300 mL of deionized water. Add tris(hydroxymethyl)aminomethane at a drop rate of 1 drop / s to adjust the pH value to 8, then add 3 mL of tetraethyl orthosilicate. Stir the mixture at a stirring speed of 200 r / min for 6 hours and then age it for 2 hours. Then add 0.3 g of silane coupling agent KH-570 and continue stirring the reaction for 3 hours. After filtering, the precipitate is washed 3 times with deionized water and 3 times with ethanol in turn to obtain the wear-resistant modified component.
[0027] A method for preparing a flame retardant and wear-resistant protective film, the preparation method comprising: S1. Weigh 100 parts of flame-retardant polyurethane emulsion, 6 parts of auxiliary flame-retardant component, 10 parts of wear-resistant modified component and 2 parts of silane coupling agent KH-560 according to weight, mix them, stir at a stirring speed of 200 r / min for 30 minutes, and record them as emulsion components; S2. Pour the emulsion components into a polytetrafluoroethylene mold, dry it at room temperature for 7 days, and then dry it in a vacuum drying oven at 60°C for 4 hours to obtain a flame retardant and wear-resistant protective film.
[0028] Example 3
[0029] A flame retardant and wear-resistant protective film of this embodiment, the flame retardant and wear-resistant protective film is composed of the following components: flame retardant polyurethane emulsion, auxiliary flame retardant component, wear-resistant modified component and silane coupling agent KH-560; The flame retardant polyurethane emulsion is prepared from phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dimethylol propionic acid as raw materials, wherein the preparation method of the flame retardant polyurethane emulsion is as follows: S2.1. Weigh 6 g of phosphorus-containing polyol, 20 g of polypropylene glycol, 15 g of toluene diisocyanate and 4 g of 2,2-dimethylol propionic acid into a flask, react at 85°C for 2 h under nitrogen protection, then add 8 g of N'N-bis(2-hydroxymethyl)aminoethylphosphonic acid dimethyl ester at a rate of 1 drop / s, then add 20 mL of butanone, continue to react for 2 h, then add 3 g of triethylamine and react again for 10 min. The result is recorded as the prepolymer component. S2.2. Pour the prepolymer and 45 mL of deionized water into a high-speed shearing machine and shear at a speed of 1000 r / min for 4 minutes. After removing butanone by rotary evaporation at a temperature of 65°C, the resulting flame-retardant polyurethane emulsion is obtained.
[0030] The auxiliary flame retardant component is prepared by modifying ammonium polyphosphate with graphene oxide, wherein the preparation method of the auxiliary flame retardant component is: S4.1. Weigh 7 g of ammonium polyphosphate and 0.5 g of silane coupling agent KH-550 and disperse them in 100 mL of anhydrous ethanol. Stir the mixture in a water bath at 100 °C at a stirring speed of 300 r / min for 5 h. The result is recorded as the reaction system. Weigh 1 g of graphene oxide and disperse it in 1 L of deionized water. Ultrasonic dispersion is performed at a frequency of 28 kHz for 10 min and recorded as the graphene oxide dispersion. S4.2. Add 20 mL of graphene oxide dispersion into the reaction system, and then place it in a water bath at 100°C and stir at a speed of 400 r / min for 5 hours. Wash the solid product with deionized water 5 times and then freeze-dry it to obtain the auxiliary flame retardant component.
[0031] The wear-resistant modified component is prepared by using dopamine-modified boron nitride and tetraethyl orthosilicate as raw materials, wherein the preparation method of the wear-resistant modified component is as follows: S6.1. Weigh 3 g of boron nitride and disperse it in 1 L of isopropanol. Ultrasonicate at 200 W for 24 h and centrifuge at 4000 r / min for 10 min. Take the upper suspension and centrifuge at 8000 r / min for 10 min. The supernatant is naturally air-dried and recorded as pretreated boron nitride. S6.2, weigh 3g of pretreated boron nitride and disperse it in 400mL of deionized water, add 0.5g of dopamine hydrochloride after ultrasonic oscillation at a power of 200W for 5h, add tris(hydroxymethyl)aminomethane at a rate of 1 drop / s under stirring at a speed of 300r / min to adjust the pH value to 7.8, and finally react at a temperature of 70°C for 5h, and filter to obtain dopamine-modified boron nitride; S6.3. Weigh 3 g of dopamine-modified boron nitride and disperse it in 300 mL of deionized water. Add tris(hydroxymethyl)aminomethane at a drop rate of 1 drop / s to adjust the pH value to 8, then add 3 mL of tetraethyl orthosilicate. Stir the mixture at a stirring speed of 200 r / min for 6 hours and then age it for 2 hours. Then add 0.3 g of silane coupling agent KH-570 and continue stirring the reaction for 3 hours. After filtering, the precipitate is washed 3 times with deionized water and 3 times with ethanol in turn to obtain the wear-resistant modified component.
[0032] A method for preparing a flame retardant and wear-resistant protective film, the preparation method comprising: S1. Weigh 100 parts of flame-retardant polyurethane emulsion, 6 parts of auxiliary flame-retardant component, 9 parts of wear-resistant modified component and 2 parts of silane coupling agent KH-560 according to weight, mix them, stir at a stirring speed of 200 r / min for 30 minutes, and record them as emulsion components; S2. Pour the emulsion components into a polytetrafluoroethylene mold, dry it at room temperature for 7 days, and then dry it in a vacuum drying oven at 60°C for 4 hours to obtain a flame retardant and wear-resistant protective film.
[0033] Comparative Example 1 The flame-retardant and wear-resistant protective film and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 1, the flame-retardant polyurethane emulsion in Example 1 is replaced with an aqueous polyurethane emulsion.
[0034] Comparative Example 2 The flame retardant and wear-resistant protective film and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 2, the auxiliary flame retardant component in Example 1 is replaced with ammonium polyphosphate.
[0035] Comparative Example 3 The flame retardant and wear-resistant protective film and the preparation method thereof provided in this comparative example are substantially the same as those in Example 1, with the main difference being that in this comparative example 3, the wear-resistant modified component in Example 1 is replaced with silicon dioxide.
[0036] Performance Testing The flame retardant and wear resistant protective films in Examples 1-3 and Comparative Examples 1-3 are marked as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3, respectively. Then, the performance of Examples 1-3 and Comparative Examples 1-3 is tested. The specific testing methods and test items are as follows: 1. The samples in Examples 1-3 and Comparative Examples 1-3 were cut into a size of 120×60×1 mm3, and the limiting oxygen index of the samples was tested respectively. The obtained data are recorded in the following table; 2. The wear resistance of the flame retardant and wear-resistant protective film in Examples 1-3 and Comparative Examples 1-3 was tested using a wear tester. The wear resistance grades were 1-5, and the wear resistance grades from 1 to 5 were getting higher and higher, and the wear resistance effect was getting better and better. The wear resistance grade of less than 30,000 friction times was 1, the wear resistance grade of 30,000-60,000 friction times was 2, the wear resistance grade of 60,000-90,000 friction times was 3, the wear resistance grade of 90,000-120,000 friction times was 4, and the wear resistance grade of more than 120,000 friction times was 5. The obtained data are recorded in the following table; 3. The mechanical properties of the flame retardant and wear resistant protective films in Examples 1-3 and Comparative Examples 1-3 were tested with reference to the standard of QB-T2415-1998, including tensile strength and elongation at break, and the obtained data are recorded in the following table; Test items Limiting oxygen index% Wear resistance grade Tensile strength MPa Elongation at break % Example 1 24.9 5 15.6 530 Example 2 23.5 5 14.9 520 Example 3 24.1 5 15.2 510 Comparative Example 1 17.6 5 13.8 450 Comparative Example 2 18.5 4 14.1 430 Comparative Example 3 22.9 2 14.5 440 It can be seen from the data in the above table that the flame retardant properties of the flame retardant and wear-resistant protective film in the present embodiments 1-3 are significantly better than those in the comparative examples 1-2, indicating that the flame retardant polyurethane emulsion and the auxiliary flame retardant components added in the present embodiments 1-3 can cooperate with each other, so that the prepared flame retardant and wear-resistant protective film has more stable flame retardant properties; secondly, the wear resistance of the flame retardant and wear-resistant protective film in the present embodiments 1-3 is significantly better than that in the comparative example 3, indicating that the wear-resistant modified components added in the embodiments 1-3 can have a better wear-resistant effect, so that the flame retardant and wear-resistant protective film prepared in the present invention has excellent flame retardant and wear-resistant properties.
[0037] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0038] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A flame retardant and wear-resistant protective film, characterized in that: The flame retardant and wear-resistant protective film is composed of the following components: flame retardant polyurethane emulsion, auxiliary flame retardant component, wear-resistant modified component and silane coupling agent KH-560; The flame retardant polyurethane emulsion is prepared using phosphorus-containing polyol, polypropylene glycol, toluene diisocyanate and 2,2-dimethylol propionic acid as raw materials; The auxiliary flame retardant component is prepared by modifying ammonium polyphosphate with graphene oxide; The wear-resistant modified component is prepared by using dopamine-modified boron nitride and tetraethyl orthosilicate as raw materials.
2. The flame retardant and wear resistant protective film according to claim 1, characterized in that: The preparation method of the flame retardant polyurethane emulsion is: S2.
1. Weigh 5-6g of phosphorus-containing polyol, 19-20g of polypropylene glycol, 15-16g of toluene diisocyanate and 3-4g of 2,2-dimethylol propionic acid into a flask, react at 85°C for 2h under nitrogen protection, dropwise add 8g of N'N-bis(2-hydroxymethyl)aminoethylphosphonic acid dimethyl ester and then add 20mL of butanone, continue to react for 2h, add 2-3g of triethylamine and react again for 10min, the obtained product is recorded as the prepolymer component; S2.
2. Pour the prepolymer and 40-50 mL of deionized water into a high-speed shearing machine for high-speed shearing. After removing butanone by rotary evaporation, the resulting flame-retardant polyurethane emulsion is obtained.
3. The flame retardant and wear resistant protective film according to claim 2, characterized in that: The dripping rate in S2.1 is 1 drop / s, the specific operation of high-speed shearing in S2.2 is shearing at a rotation speed of 1000 r / min for 3-5 min, and the temperature of the rotary evaporation in S2.2 is 65°C.
4. The flame retardant and wear resistant protective film according to claim 1, characterized in that: The preparation method of the auxiliary flame retardant component is: S4.
1. Weigh 7 g of ammonium polyphosphate and 0.5 g of silane coupling agent KH-550 and disperse them in 100 mL of anhydrous ethanol. Stir and react for 5 h in a water bath at 100 °C. The result is recorded as the reaction system. Weigh 1 g of graphene oxide and disperse it in 1 L of deionized water. After ultrasonic dispersion, it is recorded as the graphene oxide dispersion. S4.
2. Add 20 mL of graphene oxide dispersion into the reaction system, then place it in a water bath at 100°C and stir the reaction for 5 hours. Wash the solid product with deionized water 5 times and then freeze-dry it to obtain the auxiliary flame retardant component.
5. The flame retardant and wear resistant protective film according to claim 4, characterized in that: The stirring speed of the stirring reaction in S4.1 is 300 r / min, the specific operation of ultrasonic dispersion in S4.1 is ultrasonic dispersion at a frequency of 28 kHz for 10 min, and the stirring speed of the stirring reaction in S4.2 is 400 r / min.
6. The flame retardant and wear resistant protective film according to claim 1, characterized in that: The preparation method of the wear-resistant modified component is: S6.
1. Weigh 3 g of boron nitride and disperse it in 1 L of isopropanol. After ultrasonic oscillation, perform the first centrifugation. Take the upper suspension and perform the second centrifugation. The obtained supernatant is naturally air-dried and recorded as pretreated boron nitride. S6.2, weigh 3g of pretreated boron nitride and disperse it in 400mL of deionized water, add 0.5g of dopamine hydrochloride after ultrasonic oscillation, add tris(hydroxymethyl)aminomethane dropwise under stirring to adjust the pH value to 7.8, and finally react at 70°C for 5h, and filter to obtain dopamine-modified boron nitride; S6.
3. Weigh 3 g of dopamine-modified boron nitride and disperse it in 300 mL of deionized water. Add tris(hydroxymethyl)aminomethane) to adjust the pH value to 8, then add 3 mL of tetraethyl orthosilicate. Stir the reaction for 6 hours and then age it for 2 hours. Then add 0.3 g of silane coupling agent KH-570 and continue stirring the reaction for 3 hours. After filtering, the precipitate is washed 3 times with deionized water and 3 times with ethanol to obtain the wear-resistant modified component.
7. The flame retardant and wear resistant protective film according to claim 6, characterized in that: In S6.1, the specific operation of ultrasonic oscillation is ultrasonic oscillation at a power of 200 W for 24 hours, the specific operation of the first centrifugation is centrifugation at a speed of 4000 r / min for 10 minutes, and the specific operation of the second centrifugation is centrifugation at a speed of 8000 r / min for 10 minutes.
8. The flame retardant and wear resistant protective film according to claim 6, characterized in that: In S6.2, the specific operation of ultrasonic oscillation is ultrasonic oscillation at a power of 200 W for 5 hours, the stirring speed of the stirring conditions is 300 r / min, and the dripping rate is 1 drop / s. In S6.3, the stirring speed of the stirring reaction is 200 r / min, and the dripping rate is 1 drop / s.
9. A method for preparing a flame retardant and wear resistant protective film according to any one of claims 1 to 8, characterized in that: The preparation method is: S1. Weigh 100 parts of flame-retardant polyurethane emulsion, 5-6 parts of auxiliary flame-retardant component, 8-10 parts of wear-resistant modification component and 1-2 parts of silane coupling agent KH-560 according to weight, mix them, and record them as emulsion components after mixing and dispersing them evenly; S2. Pour the emulsion components into a polytetrafluoroethylene mold, and after drying, obtain a flame retardant and wear-resistant protective film.
10. The method for preparing a flame retardant and wear resistant protective film according to claim 9, characterized in that: The specific operation of mixing and dispersing uniformly in S1 is stirring at a stirring speed of 200 r / min for 30 minutes, and the specific operation of drying treatment in S2 is: first drying at room temperature for 7 days, and then placing in a vacuum drying oven at 60° C. to dry for 4 hours.
Citation Information
Patent Citations
Halogen free phosphorous-nitrogen synergic antiflaming water-soluble polyurethane fabric coating agent and preparation method thereof
CN101982603A
Environmentally-friendly halogen-free reaction type soft and hard segment co-modified flame retardant waterborne polyurethane fabric coating agent and preparation method thereof
CN102226314A
Anti-flaming water-borne polyurethane and preparation method thereof, and adhesive and preparation method thereof
CN106750175A
Ammonium polyphosphate-waste PCB powder modified flame retardant polypropylene based plate and preparation method thereof
CN107163390A
Cited By
Protective film, preparation method thereof and lithium ion battery
CN121439997A