A pretreatment process for synthesizing bisphenol A resin catalyst

Through the continuous treatment method of purging and venting, standing displacement and rinsing, and taking advantage of the gradient difference of phenol aqueous solution, the water content in the resin catalyst was successfully reduced, solving the problems of long pretreatment time and large amount of phenol in the existing technology, and realizing Efficient water content control and cost reduction.

CN118253111BActive Publication Date: 2024-10-25TIANJIN UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410481158.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2024-10-25
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

In the prior art, the pretreatment process for catalytically synthesizing bisphenol A resin catalysts has problems such as long processing time, large dosage of phenol, and difficulty in controlling the water content in the resin catalyst. In particular, there are no strict definition standards and effective pretreatment operation plans.

Method used

Continuous treatment methods of purging, venting, standing replacement, and washing are adopted, and phenol aqueous solutions with different concentration gradients are used to stand standing replacement and elution of the resin catalyst, and the physically bound water and unbound water in the resin catalyst bed are discharged, and the resin catalyst is reduced Water content of the catalyst.

Benefits of technology

The water content of the resin catalyst can be reduced quickly and with low phenol dosage. The pretreatment time is short and the cost is reduced. The water content in the resin catalyst is less than 1.0% by weight, which meets the requirements of catalytic performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118253111B_ABST
    Figure CN118253111B_ABST
Patent Text Reader

Abstract

The present invention provides a pretreatment process for synthesizing a bisphenol A resin catalyst. First, the resin catalyst is purged with gas to drain the residual liquid in the resin catalyst; then, the emptied resin catalyst is contacted with a replacement washing liquid, and the replacement is allowed to stand for static replacement, and the replacement washing liquid is drained; then, the resin catalyst obtained above is contacted with the replacement washing liquid, and the replacement is allowed to stand for static replacement; finally, the eluent is contacted with the resin catalyst, and the eluent is drained to obtain the pretreated resin catalyst. The water in the catalytic synthesis of bisphenol A resin catalyst is effectively removed, and the water content in the resin catalyst is less than 1.0 weight percent; the amount of phenol used in the washing liquid is reduced, the material consumption and energy consumption are reduced, and the cost of the pretreatment process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a resin catalyst pretreatment process for catalyzing the synthesis of bisphenol A by a resin catalyst, and in particular to a process for reducing the water content in a catalytic bisphenol A resin catalyst. Background Art

[0002] Bisphenol A (BPA), chemical name 2,2-bis(4-hydroxyphenyl)propane, is a widely used organic chemical raw material made by condensation of phenol and acetone under the action of a catalyst. It is mainly used in the production of polycarbonate, epoxy resin and other polymer materials.

[0003] The ion exchange resin method for synthesizing bisphenol A has a simple process flow, low corrosion to equipment, and low discharge of three wastes, and has been widely used in industry. The catalyst used in this method is an ion exchange resin obtained by sulfonation or thiol modification with styrene or substituted styrene as a monomer, divinylbenzene as a cross-linking agent, and liquid paraffin as a porogen, and has the characteristics of high catalytic activity and good selectivity. Although the ion exchange resin catalyst has a smooth pore structure and a suitable acid amount and acid strength, the synthetic monomers, cross-linking agents and porogens remaining in the resin during the preparation process will cause side reactions to occur, and even block the pores, thereby affecting the catalytic performance. In addition, the remaining water in the ion exchange resin will cause the equilibrium of the bisphenol A synthesis reaction to move in the reverse direction, reducing the conversion rate of the synthesis reaction. At the same time, water will occupy the active center of the catalyst, causing the catalytic activity to decrease, resulting in a decrease in the reaction rate. For this reason, the ion exchange resin needs to be pretreated before use to remove the residues and water in the resin synthesis.

[0004] Patent CN100546963C invented an industrial-scale continuous production method for forming bisphenol by reacting ketone with phenol, in which phenol and ketone are directly contacted with a modified ion exchange resin catalyst and reacted to obtain bisphenol. Patent CN1150150C invented a method for preparing bisphenol A, in which phenol and acetone are directly contacted with an acidic ion exchange resin catalyst and an alkyl mercaptan co-catalyst to obtain bisphenol A. CN103974925B invented a method for preparing diphenol 2,2-bis(4′-hydroxyphenyl)propane, in which an antioxidant is contacted with an ion exchange resin catalyst before phenol and acetone react with the catalyst to form a treated and promoted catalyst, thereby improving the stability and catalytic reaction performance of the catalyst. However, in the reports on these bisphenol A production methods, there is no mention of methods and standard requirements for reducing water content and activation of the resin pretreatment, which are key factors affecting the efficient catalytic synthesis of bisphenol A and catalytic stability of the resin catalyst.

[0005] At present, the pretreatment method of the catalyst for catalytic synthesis of bisphenol A resin in industry is to use the reactant phenol as a washing liquid, inject it into a fixed bed reactor filled with the resin catalyst, contact it with the resin catalyst, and replace or wash the residue and water in the resin. Although this method can remove the residue and water in the resin, it takes a long time to operate, uses a large amount of phenol washing liquid, has a high pretreatment cost, and it is difficult to reduce the water content of the resin to less than 1.0 weight%.

[0006] In summary, in the current process of synthesizing bisphenol A using resin catalysts, the resin catalyst pretreatment process is not considered, and in particular, there is no strict limit standard and effective resin pretreatment operation scheme for controlling the water content in the resin catalyst before the reaction. Therefore, it is necessary to develop a resin catalyst pretreatment process for synthesizing bisphenol A using resin catalysts, reduce the time of the pretreatment process, reduce the amount of washing liquid used in the pretreatment, and quickly reduce the water content in the resin catalyst to less than 1.0 weight %.

[0007] To this end, the present invention aims at the problems of long treatment time, large amount of phenol, and difficult to control water content in resin catalyst during the pretreatment of catalytic bisphenol A resin catalyst, and develops a new resin catalyst pretreatment method and a matching, suitable phenol concentration and phenol amount. The main innovation is: a continuous treatment method using purging, venting, static replacement, and washing is proposed, and the resin is statically replaced and washed using phenol aqueous solutions with different concentration gradients to discharge physically bound water (bound water) inside the resin catalyst particles in the resin catalyst bed and unbound water that is strongly bound to the resin catalyst and difficult to desorb. Summary of the invention

[0008] The purpose of the present invention is to provide a resin catalyst pretreatment process for catalyzing the synthesis of bisphenol A by a resin catalyst, wherein the residual liquid in the resin catalyst is emptied and then a static replacement method is adopted: the resin catalyst after being emptied in a fixed bed reactor is used as a replaced object and is in a static state relative to the reactor; phenol is used as a replacement liquid to contact the resin catalyst, enter the internal pore structure of the replaced object, and replace the water in the pores of the replaced object.

[0009] The resin catalyst after being emptied is contacted with the replacement washing liquid, the replacement washing liquid is emptied, and the static replacement method is continued to be adopted to contact the resin after static replacement with the replacement washing liquid, and finally the elution method is adopted to contact the elution liquid with the resin catalyst, and the elution liquid is emptied to obtain a resin catalyst with a low water content. The process technology can quickly and effectively remove water from the catalyst for catalytic synthesis of bisphenol A resin, the resin pretreatment time is short, and the amount of washing liquid used is small.

[0010] In order to achieve the purpose of the present invention, the technical solution adopted by the present invention is as follows:

[0011] A resin catalyst pretreatment process for synthesizing bisphenol A catalyzed by a resin catalyst comprises the following steps:

[0012] (a) draining the residual liquid in the resin catalyst: using a purge gas to purge the resin catalyst to drain the residual liquid in the resin catalyst;

[0013] (b) using a static displacement method, contacting the emptied resin catalyst with a displacement washing liquid, static displacement, and draining the displacement washing liquid;

[0014] (c) contacting the resin catalyst obtained above with the replacement washing liquid by static replacement method, and static replacement;

[0015] (d) using an elution method to contact the eluent with the resin catalyst, and draining the eluent to obtain a pretreated resin catalyst;

[0016] The replacement washing solutions in the above steps (c) and (b) are both phenol aqueous solutions, but the phenol concentration in the phenol aqueous solution in step (c) is higher than that in step (b).

[0017] The resin catalyst pretreatment process for synthesizing bisphenol A by resin catalysis, the step (a) specifically comprises: passing a purge gas from an upper gas inlet into a fixed bed reactor, contacting the purge gas with the resin catalyst, removing liquid from the resin catalyst, and obtaining a vented resin catalyst, the purge gas being discharged from a lower gas outlet of the fixed bed reactor;

[0018] (b) Specifically, the outlet of the fixed bed reactor is closed, and the replacement washing liquid is introduced into the fixed bed reactor from the washing liquid inlet, contacted with the resin catalyst, and statically replaced. After the static replacement is completed, the washing liquid outlet of the fixed bed reactor is opened, and the purge gas is introduced to discharge the washing liquid from the bottom outlet of the fixed bed;

[0019] (c) Specifically, the outlet of the fixed bed reactor is closed, and the replacement washing liquid is introduced into the fixed bed reactor from the washing liquid inlet to contact with the resin catalyst and stand for replacement;

[0020] (d) Specifically, the eluent is introduced into the fixed bed reactor from the washing liquid inlet to contact and elute the resin catalyst, and the washing liquid outlet of the fixed bed reactor is opened to discharge the eluent to obtain the pretreated resin catalyst.

[0021] In the above technical solution, the resin catalyst is an acidic ion exchange resin, which is a gel type or a macroporous type, with a resin crosslinking degree of 1.0% to 20%, a particle size range of 0.4nm to 5.0nm, and a water content of 20% to 90% by weight.

[0022] In the above technical scheme, the step (a) uses a purge gas to purge the residual liquid in the resin catalyst, the purge gas enters from the upper part of the resin catalyst bed, and the residual liquid and tail gas are discharged from the lower part of the resin catalyst bed. The purge gas is one or more combinations of air, ethane, propane, nitrogen, argon or helium.

[0023] In the above technical solution, the purge gas temperature in step (a) is 40°C to 80°C, the purge gas flow rate per minute is 1 to 5 times the resin catalyst loading volume, and the purge time is 10 to 120 minutes.

[0024] In the above technical scheme, the temperature of the resin catalyst bed in the static displacement in step (b) is 45°C to 95°C; the phenol content of the displacement washing liquid is 10 to 95% by weight, the temperature of the displacement washing liquid is 45°C to 95°C, the amount of the displacement washing liquid is 0.5 to 3 times the volume of the resin catalyst loading, and the standing time is 0.5 hour to 24 hours.

[0025] In the above technical scheme, the purge gas in step (b) is one or more combinations of air, ethane, propane, nitrogen, argon or helium, the purge gas temperature is 40°C to 80°C, the purge gas flow rate per minute is 1 to 5 times the resin catalyst loading volume, and the purge time is 10 to 120 minutes.

[0026] In the above technical scheme, the temperature of the resin catalyst bed in the static displacement in step (c) is 45°C to 95°C; the phenol content of the displacement washing liquid is 80 to 99.5 weight %; the temperature of the displacement washing liquid is 45°C to 95°C, the amount of the displacement washing liquid is 0.5 to 3 times the volume of the resin catalyst loading, and the standing time is 0.5 hour to 24 hours.

[0027] In the above technical solution, the eluent in step (d) is phenol, and the temperature of the eluent is 45°C to 95°C.

[0028] In the above technical solution, the hourly flow rate of the elution liquid in step (d) is 0.05 to 0.2 times the loading volume of the resin catalyst, and the elution time is 0.5 to 72 hours.

[0029] The present invention solves the following problems:

[0030] 1. In view of the problems of long treatment time, large amount of phenol and difficult to control water content in the resin during the pretreatment of catalytic bisphenol A resin catalyst, we have developed a new resin catalyst pretreatment method and its matching, suitable phenol concentration and phenol dosage. The main innovation is: a continuous treatment method using purging, venting, static replacement and washing is proposed, and the resin catalyst is statically replaced and washed using phenol aqueous solutions with different concentration gradients;

[0031] 2. From the literature reports, there is no report on the resin pre-catalyst treatment process in the process of bisphenol A catalyzed by resin catalyst. At present, in industrial practice, before the resin catalyzed synthesis of bisphenol A, the phenol in the bisphenol A reaction is usually contacted with the resin catalyst to remove water from the resin catalyst. In this patent invention, we propose to use a continuous treatment method of purging, venting, static replacement, and washing to pre-treat and dehydrate the resin catalyst.

[0032] 3. The principle of the invention of this patent: In the continuous treatment method of purging, venting, static replacement, and washing, ① purging and venting process: discharge the water between the resin catalyst particles in the resin catalyst bed; ② static replacement process: in this process, the replacement liquid phenol aqueous solution enters the interior of the resin catalyst particles in the resin catalyst bed, replaces and discharges the physically bound water (bound water) inside the resin catalyst particles in the resin catalyst bed, and at the same time, the concentration gradient difference of the phenol aqueous solution in the replacement liquid is used to control the resin bed so that the porous structure inside the resin does not shrink or even collapse due to excessive and rapid dehydration; ③ washing process: in this process, the washing liquid phenol enters the interior of the resin catalyst particles in the resin catalyst bed, and the concentration difference between the phenol in the washing liquid and the phenol in the resin catalyst is used to remove the resin (the resin is formed by the polymerization and cross-linking of styrene and diphenylethylene, in which vinyl and phenyl groups are more likely to interact strongly with water) with strong binding and difficult to desorb (non-bound water). In summary, the resin catalyst pretreatment process proposed in the present invention utilizes a continuous treatment method of purging, venting, static replacement, and washing and a concentration gradient difference of the washing liquid to sequentially remove bound water and unbound water in the resin catalyst bed, and quickly and with a low phenol dosage, achieves a reduction in water content in the resin catalyst while ensuring that the pore structure and chemical properties of the resin bed remain unchanged.)

[0033] The advantages and beneficial effects of the present invention are as follows:

[0034] (1) The present invention relates to a new pretreatment process for a catalyst for catalytic synthesis of bisphenol A resin, which is characterized in that a resin catalyst pretreatment dehydration process is invented, which can quickly remove water from the catalyst for catalytic synthesis of bisphenol A resin, and the resin catalyst pretreatment time is short.

[0035] (2) The present invention relates to a new pretreatment process for catalytic synthesis of bisphenol A resin catalyst, which is characterized in that a resin catalyst pretreatment dehydration process is invented, which can reduce the amount of phenol used in the washing liquid, reduce material consumption and energy consumption, and reduce the cost of the pretreatment process.

[0036] (3) The present invention relates to a new pretreatment process for a catalyst for catalytic synthesis of bisphenol A resin, which is characterized in that a resin catalyst pretreatment dehydration process is invented, which can effectively remove water from the catalyst for catalytic synthesis of bisphenol A resin, and the water content in the resin catalyst is less than 1.0 weight%. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The present invention is a simplified flow chart of the resin catalyst pretreatment technology scheme for catalytic synthesis of bisphenol A. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below with reference to the accompanying drawings and through specific embodiments. The following embodiments are merely illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0039] The following uses specific examples to illustrate the specific implementation process of the method of this application.

[0040] Example 1

[0041] Step (a), 1 liter of gel-type ion exchange resin catalyst (crosslinking degree 4%, particle size range 0.6-1.5nm, water content 60% by weight) is loaded into a fixed bed reactor, and the resin catalyst bed temperature is preheated to 50° C. During the pretreatment process, the resin catalyst bed temperature is maintained at 50° C. The outlet valve below the fixed bed reactor is opened, nitrogen (nitrogen flow rate 2 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 30 minutes, the outlet valve below the fixed bed is closed.

[0042] Step (b), 1.5 liters of phenol aqueous solution (phenol content 10 wt%) was then preheated to 50° C., added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 50° C. and allowed to stand for 5 hours. The outlet valve below the fixed bed reactor was opened, nitrogen (nitrogen flow rate 2 liters / minute) was introduced from above the fixed bed, the standing liquid was discharged from the bottom outlet of the fixed bed, purged for 30 minutes, and the outlet valve below the fixed bed was closed.

[0043] Step (c), then preheat 1.5 liters of phenol aqueous solution (phenol content 99.5 wt%) to 50°C, add it to the fixed bed to contact with the resin catalyst, and keep the resin catalyst bed at 50°C and let it stand for 5 hours.

[0044] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 50° C., phenol addition amount is 0.05 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 24 hours to obtain a pretreated resin catalyst.

[0045] According to the method of this embodiment, the resin catalyst is pretreated for 35 hours. After the treatment, the water content of the resin catalyst is reduced to 0.93% by weight, meeting the pretreatment requirement of the resin catalyst water content being lower than 1.0% by weight.

[0046] Example 2

[0047] Step (a), 1 liter of gel-type ion exchange resin catalyst (crosslinking degree 8%, particle size range 0.4-1.5nm, water content 30% by weight) is loaded into a fixed bed reactor, and the resin catalyst bed temperature is preheated to 70° C. During the pretreatment process, the resin catalyst bed temperature is maintained at 70° C. The outlet valve below the fixed bed reactor is opened, air (air flow rate 2.5 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 60 minutes, the outlet valve below the fixed bed is closed.

[0048] Step (b), 1.5 liters of phenol aqueous solution (phenol content 95 wt%) was then preheated to 70° C., added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 70° C. and allowed to stand for 4 hours. The outlet valve below the fixed bed reactor was opened, air (air flow rate 2.5 liters / minute) was introduced from above the fixed bed, the standing liquid was discharged from the bottom outlet of the fixed bed, purged for 60 minutes, and the outlet valve below the fixed bed was closed.

[0049] Step (c), then preheat 1.5 liters of phenol aqueous solution (phenol content 98.5 wt%) to 70°C, add it to the fixed bed to contact with the resin catalyst, and keep the resin catalyst bed at 70°C for 4 hours.

[0050] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 70° C., phenol addition amount is 0.1 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 20 hours to obtain a pretreated resin catalyst.

[0051] According to the method of this embodiment, the resin catalyst is pretreated for 30 hours. After the treatment, the water content of the resin catalyst is reduced to 0.95% by weight, meeting the pretreatment requirement of the resin catalyst water content being lower than 1.0% by weight.

[0052] Example 3

[0053] Step (a), 1 liter of macroporous ion exchange resin catalyst (crosslinking degree 6%, particle size range 0.8-2.0nm, water content 65% by weight) is loaded into a fixed bed reactor, and the resin catalyst bed temperature is preheated to 45° C. During the pretreatment process, the resin catalyst bed temperature is maintained at 45° C. The outlet valve below the fixed bed reactor is opened, nitrogen (argon flow rate 2 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 30 minutes, the outlet valve below the fixed bed is closed.

[0054] Step (b), 2 liters of phenol aqueous solution (phenol content 52.5 wt%) was then preheated to 45°C, added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 45°C and allowed to stand for 4 hours. The outlet valve below the fixed bed reactor was opened, nitrogen (argon flow rate 2 liters / minute) was introduced from above the fixed bed, the standing liquid was discharged from the bottom outlet of the fixed bed, purged for 30 minutes, and the outlet valve below the fixed bed was closed.

[0055] Step (c), then preheating 2 liters of phenol aqueous solution (phenol content 80% by weight) to 45°C, adding it to the fixed bed to contact with the resin catalyst, and maintaining the resin catalyst bed at 45°C for 8 hours.

[0056] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 45° C., phenol addition amount is 0.15 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 20 hours to obtain a pretreated resin catalyst.

[0057] According to the method of this embodiment, the resin catalyst was pretreated for 33 hours. After the treatment, the water content of the resin catalyst dropped to 0.92% by weight, meeting the pretreatment requirement of the resin catalyst water content being lower than 1.0% by weight.

[0058] Example 4

[0059] Step (a), 1 liter of macroporous ion exchange resin catalyst (crosslinking degree 10%, particle size range 0.5-1.2nm, water content 25% by weight) is loaded into a fixed bed reactor, and the resin catalyst bed temperature is preheated to 90° C. During the pretreatment process, the resin catalyst bed temperature is maintained at 90° C. The outlet valve below the fixed bed reactor is opened, nitrogen (nitrogen flow rate 1.5 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 30 minutes, the outlet valve below the fixed bed is closed.

[0060] Step (b), 2.5 liters of phenol aqueous solution (phenol content 75 wt%) was then preheated to 90° C., added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 90° C. and allowed to stand for 3 hours. The outlet valve below the fixed bed reactor was opened, nitrogen (nitrogen flow rate 1.5 liters / minute) was introduced from above the fixed bed, the stationary liquid was discharged from the bottom outlet of the fixed bed, purged for 30 minutes, and the outlet valve below the fixed bed was closed.

[0061] Step (c), then preheat 1.5 liters of phenol aqueous solution (phenol content 90% by weight) to 90° C., add it to the fixed bed to contact with the resin catalyst, and keep the resin catalyst bed at 90° C. and let it stand for 3 hours.

[0062] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 90° C., phenol addition amount is 0.125 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 21 hours to obtain a pretreated resin catalyst.

[0063] According to the method of this embodiment, the resin catalyst is pretreated for 28 hours. After the treatment, the water content of the resin catalyst is reduced to 0.90% by weight, meeting the pretreatment requirement of the resin catalyst having a water content of less than 1.0% by weight.

[0064] Example 5

[0065] Step (a), 1 liter of gel-type ion exchange resin catalyst (crosslinking degree 10%, particle size range 0.5-1.2nm, water content 27% by weight) is loaded into a fixed bed reactor, and the resin catalyst bed temperature is preheated to 80° C. During the pretreatment process, the resin catalyst bed temperature is maintained at 80° C. The outlet valve below the fixed bed reactor is opened, helium (helium flow rate 2.5 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 60 minutes, the outlet valve below the fixed bed is closed.

[0066] Step (b), 2.0 liters of phenol aqueous solution (phenol content 80 wt%) was then preheated to 80° C., added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 80° C. and allowed to stand for 4 hours. The outlet valve below the fixed bed reactor was opened, helium (helium flow rate 2.5 liters / minute) was introduced from above the fixed bed, the stationary liquid was discharged from the bottom outlet of the fixed bed, purged for 60 minutes, and the outlet valve below the fixed bed was closed.

[0067] Step (c), then preheat 2.0 liters of phenol aqueous solution (phenol content 95% by weight) to 80°C, add it to the fixed bed to contact with the resin catalyst, and keep the resin catalyst bed at 80°C for 4 hours.

[0068] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 80° C., phenol addition amount is 0.2 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 20 hours to obtain a pretreated resin catalyst.

[0069] According to the method of this embodiment, the resin catalyst is pretreated for 30 hours. After the treatment, the water content of the resin catalyst is reduced to 0.98% by weight, meeting the pretreatment requirement of the resin catalyst water content being lower than 1.0% by weight.

[0070] Example 6

[0071] Step (a), 1 liter of gel-type ion exchange resin catalyst (crosslinking degree 6%, particle size range 1.2-2.5 nm, water content 40 wt%) is loaded into a fixed bed reactor, the resin catalyst bed temperature is preheated to 65° C., and the resin catalyst bed temperature is maintained at 65° C. during the pretreatment process. The outlet valve below the fixed bed reactor is opened, nitrogen (nitrogen flow rate 2.5 liters / minute) is introduced from above the fixed bed, residual liquid is discharged from the bottom outlet of the fixed bed, and after purging for 30 minutes, the outlet valve below the fixed bed is closed.

[0072] Step (b), 2.0 liters of phenol aqueous solution (phenol content 70 wt%) was then preheated to 65° C., added to the fixed bed to contact with the resin catalyst, and the resin catalyst bed was kept at 65° C. and allowed to stand for 6 hours. The outlet valve below the fixed bed reactor was opened, nitrogen (nitrogen flow rate 2.5 liters / minute) was introduced from above the fixed bed, and the standing liquid was discharged from the bottom outlet of the fixed bed. After purging for 30 minutes, the outlet valve below the fixed bed was closed.

[0073] Step (c), then preheat 1.5 liters of phenol aqueous solution (phenol content 90% by weight) to 65° C., add it to the fixed bed to contact with the resin catalyst, and keep the resin catalyst bed at 65° C. and let it stand for 6 hours.

[0074] Step (d), open the outlet valve below the fixed bed reactor, introduce phenol from above the fixed bed (phenol temperature is 65° C., phenol addition amount is 0.2 L / h), discharge the washing liquid from the bottom outlet of the fixed bed, and rinse for 20 hours to obtain a pretreated resin catalyst.

[0075] According to the method of this embodiment, the resin catalyst was pretreated for 33 hours. After the treatment, the water content of the resin catalyst dropped to 0.96% by weight, meeting the pretreatment requirement of the resin catalyst water content being lower than 1.0% by weight.

[0076] Table 1 summarizes the embodiments of the present invention as follows, including the resin moisture content before treatment, the pretreatment time, and the resin moisture content after pretreatment. As can be seen from Table 1, when the resin moisture content after pretreatment is lower than 1.0% by weight, the resin catalyst pretreatment process described in the present invention is adopted, and the pretreatment time is 28 to 35 hours. In combination with the embodiments of the present invention, it can be seen that the resin catalyst pretreatment process described in the present invention has a short pretreatment time and a small amount of washing liquid, and the resin pretreatment requirement of less than 1.0% by weight can be achieved quickly and efficiently.

[0077] Table 1

[0078]

[0079]

[0080] Both the prior art and the inventive embodiments use phenol as a washing liquid, but the differences are: (1) In the prior art, only phenol is used to wash the resin to achieve resin dehydration, and the process takes a long time and uses a large amount of phenol; (2) The embodiments described in the present invention use a continuous treatment method of purging, venting, static displacement, and washing to pre-treat and dehydrate the resin. Specifically, the present invention uses purging and venting to discharge the water between the resin catalyst particles in the resin catalyst bed; in the static displacement process, a phenol aqueous solution is used as a displacement liquid to displace and discharge the physically bound water (bound water) inside the resin catalyst particles in the resin catalyst bed; in the washing process, the washing liquid phenol removes the (unbound water) that is strongly bound to the resin and difficult to desorb. In addition, the two methods are different in treatment conditions, washing liquid concentration, and washing liquid dosage.

[0081] From the perspective of pretreatment effect, the method described in the present invention can quickly remove water from catalytic synthesis of bisphenol A resin, and the resin pretreatment time is short; it can effectively remove water from catalytic synthesis of bisphenol A resin, and the water content in the resin is less than 1.0% by weight; this technical method has good pretreatment effect for resins with different water contents and good applicability. The water content of the resin obtained by the method described in the present invention is greatly reduced to 1.0% by weight, which can meet the requirements of catalytic performance and stability for catalytic synthesis of bisphenol A from acetone and phenol, while the untreated resin will affect the catalytic activity due to its high water content of 25-60% by weight, especially the increase in water content leads to a decrease in phenol conversion rate, a decrease in the yield of bisphenol A, and an increase in by-products, which cannot meet the requirements of industrial production. It can be seen from this that the technical necessity and advantages of the method described in the present invention are adopted.

[0082] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0083] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0084] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A pretreatment process for a resin catalyst for synthesizing bisphenol A; Its characteristics are: The steps include: (a) draining the residual liquid in the resin catalyst: using a purge gas to purge the resin catalyst to drain the residual liquid in the resin catalyst; (b) using a static displacement method, contacting the emptied resin catalyst with a displacement washing liquid, static displacement, and draining the displacement washing liquid; (c) contacting the resin catalyst obtained above with the replacement washing liquid by static replacement method, and static replacement; (d) using an elution method to contact the eluent with the resin catalyst, and draining the eluent to obtain a pretreated resin catalyst; The replacement washing solutions in the above steps (c) and (b) are both phenol aqueous solutions, but the phenol concentration in the phenol aqueous solution in step (c) is higher than that in step (b).

2. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 1; Its characteristics are: The steps (a) Specifically, the purge gas is introduced into the fixed bed reactor from the upper gas inlet to contact with the resin catalyst to remove the liquid in the resin catalyst to obtain the emptied resin catalyst, and the purge gas is discharged from the lower gas outlet of the fixed bed reactor; (b) Specifically, the outlet of the fixed bed reactor is closed, and the replacement washing liquid is introduced into the fixed bed reactor from the washing liquid inlet, contacted with the resin catalyst, and statically replaced. After the static replacement is completed, the washing liquid outlet of the fixed bed reactor is opened, and the purge gas is introduced to discharge the washing liquid from the bottom outlet of the fixed bed; (c) Specifically, the outlet of the fixed bed reactor is closed, and the replacement washing liquid is introduced into the fixed bed reactor from the washing liquid inlet to contact with the resin catalyst and stand for replacement; (d) Specifically, the eluent is introduced into the fixed bed reactor from the washing liquid inlet to contact and elute the resin catalyst, and the washing liquid outlet of the fixed bed reactor is opened to discharge the eluent to obtain the pretreated resin catalyst.

3. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: The resin catalyst is an acidic ion exchange resin, which is a gel type or a macroporous type, with a resin crosslinking degree of 1.0% to 20%, a particle size range of 0.4nm to 5.0nm, and a water content of 20% to 90% by weight.

4. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: In the step (a), the residual liquid in the resin catalyst is emptied by purging with a purge gas, the purge gas enters from the upper part of the resin catalyst bed, and the residual liquid and tail gas are discharged from the lower part of the resin catalyst bed. The purge gas is one or more combinations of air, ethane, propane, nitrogen, argon or helium.

5. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: In the step (a), the purge gas temperature is 40° C. to 80° C., the purge gas flow rate per minute is 1 to 5 times the resin catalyst loading volume, and the purge time is 10 to 120 minutes.

6. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: In the step (b) of standing displacement, the temperature of the resin catalyst bed is 45°C to 95°C; the phenol content of the displacement washing liquid is 10 to 95% by weight, the temperature of the displacement washing liquid is 45°C to 95°C, the amount of the displacement washing liquid is 0.5 to 3 times the volume of the resin catalyst loading, and the standing time is 0.5 hour to 24 hours.

7. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: The purge gas in step (b) is one or more of air, ethane, propane, nitrogen, argon or helium, the purge gas temperature is 40°C to 80°C, the purge gas flow rate per minute is 1 to 5 times the resin catalyst loading volume, and the purge time is 10 to 120 minutes.

8. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: In the step (c), the temperature of the resin catalyst bed during the static displacement is 45°C to 95°C; the phenol content of the displacement washing liquid is 80 to 99.5% by weight; the temperature of the displacement washing liquid is 45°C to 95°C, the amount of the displacement washing liquid is 0.5 to 3 times the volume of the resin catalyst loading, and the static time is 0.5 hour to 24 hours.

9. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: The eluent in step (d) is phenol, and the temperature of the eluent is 45°C to 95°C.

10. A pretreatment process for a resin catalyst for synthesizing bisphenol A as claimed in claim 2; Its characteristics are: The hourly flow rate of the elution liquid in step (d) is 0.05 to 0.2 times the loading volume of the resin catalyst, and the elution time is 0.5 to 72 hours.

Citation Information

Patent Citations

  • Process for the synthesis of bisphenol

    CN100546963C

  • Use of treated and accelerated ion exchange resin catalysts

    CN103974925B

  • Process for producing bisphenol A

    CN1150150C

  • Method to treat an ion-exchanger catalyst for the process of bisphenol-A synthesis

    CN1103396A

  • Resin catalyst for bisphenol A synthesis, preparation method of resin catalyst and bisphenol A catalytic synthesis application of resin catalyst