A kind of ultra-large straight-through pore polyethersulfone microporous filter membrane and preparation method thereof
Through high-temperature hot roll induction and steam atomization induction technology, a polyethersulfone microporous filter membrane with large pore size and through-pore structure was formed, which solved the problem of insufficient pore size and flux in the prior art, and achieved efficient water treatment effect .
Patent Information
- Application Number
- CN202410227833.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-02-29
AI Technical Summary
The pore size and flux of the existing polyethersulfone microporous filter membranes need to be improved, resulting in low separation efficiency and increased operating costs, and uneven structures, making it difficult to meet the needs of efficient water treatment.
By combining high-temperature heat roller induction and steam atomization induction, the cast film liquid is formed by adding specific solvents, additives and pore-generating agents to the cast film liquid, and the cast film liquid is formed by heat roller induction and steam atomization treatment, which is large. Polyethersulfone microporous filter membrane with pore size and through-pore structure.
The high flux and structural uniformity of the polyethersulfone microporous filter membrane were achieved, with an average pore size of 1-70μm, and the pure water flux was significantly increased to 110-840ml/cm2·min, which solved the flux and pore size in the prior art. A problem of insufficient.
Smart Images

Figure CN118253205B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of microporous filter membranes, and in particular relates to a super-large straight-through-pore polyethersulfone microporous filter membrane and a preparation method thereof. Background Art
[0002] With the rapid development of industry, the scarcity and pollution of water resources have become a major problem facing us today, and finding an efficient, economical, energy-saving, environmentally friendly and sustainable water treatment technology has become a topic that needs to be faced. Among them, membrane separation technology, as an important branch in the field of water treatment, has advantages that other types of water treatment technologies cannot match, and has always been widely concerned by people.
[0003] As a polymer membrane material with excellent comprehensive performance, polyethersulfone (PES) has high mechanical strength, excellent chemical corrosion resistance and heat resistance, and is widely used in industrial wastewater treatment, tap water purification, food processing, seawater desalination and other fields. However, the inherent hydrophobicity and dense membrane pore structure of PES make it easy to be contaminated by impurities during application, thereby reducing separation efficiency, increasing operating costs, and affecting secondary use.
[0004] For example, patent application number CN1951550A discloses a large-pore polyethersulfone membrane, a preparation method and use thereof, wherein 9-15% polyethersulfone and 5-10% additive polyvinylpyrrolidone are dissolved in 75-86% organic solvent, and the mixture is fully mixed to form a casting solution. However, the cross-section of the filter membrane prepared thereby forms finger-like pores, the structure is not uniform, and the flux is relatively small.
[0005] Patent application number CN116726724A discloses a high-flux polyethersulfone flat membrane for bacterial filtration and a preparation method thereof, wherein a uniform polymer solution is first prepared, wherein the polymer solution includes at least one volatile non-solvent, and then a high-flux polyethersulfone flat membrane for bacterial filtration is obtained by multiphase induced phase transformation, wherein the multiphase induced phase transformation includes gas phase induced phase transformation and immersion precipitation phase transformation. However, the average pore size of the polyethersulfone flat membrane prepared in this patent is 0.15-0.25 μm, and the flux is 27-32 ml / cm 2 ·min, the pore size and flux need to be improved.
[0006] Therefore, the market urgently needs to develop and prepare large-pore polyethersulfone microporous filter membranes with high flux and uniform structure. Summary of the invention
[0007] In view of this, the object of the present invention is to provide a large through-pore polyethersulfone microporous filter membrane and a preparation method thereof, which has a large pore size and a through-pore structure and has a high flux.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] The invention discloses a method for preparing a polyethersulfone microporous filter membrane with ultra-large straight-through pores, comprising the following steps:
[0010] (1) dissolving polyethersulfone in a solvent, adding additives and porogens, and mixing them uniformly to obtain a film casting solution;
[0011] (2) scraping the casting liquid to form a liquid film;
[0012] (3) After the liquid film is induced by a hot roller at 40-80°C for 5-60 seconds, it is sent to a constant temperature and humidity chamber with a humidity of 60-90% and atomized by steam at 20-45°C for 5-60 seconds;
[0013] (4) The liquid membrane after the induction treatment is solidified into a membrane in a water bath, and then cleaned and dried to obtain a polyethersulfone microporous filter membrane.
[0014] As a preferred technical solution, the solvent is one or more of butyl lactate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylformamide and dimethyl sulfoxide.
[0015] As a preferred technical solution, the additive is one or more of neopentyl glycol, diethylene glycol, dipropylene glycol, polyethylene glycol, glycolic acid and polyvinyl alcohol.
[0016] As a preferred technical solution, the porogen is polyvinyl pyrrolidone with a weight average molecular weight of 45000Da-1300000Da.
[0017] As a preferred technical solution, in step (1), the mass ratio of the solvent to polyethersulfone is 3-6:1, the mass ratio of the additive to polyethersulfone is 0.5-3:1, and the mass ratio of the porogen to polyethersulfone is 0.2-3:1.
[0018] As a preferred technical solution, in step (1), the temperature at which the polyethersulfone, solvent, additive and porogen are mixed is 50-80°C.
[0019] As a preferred technical solution, in step (2), the scraping film thickness is 100-130 μm, and the pulling speed is 1-4 m / s.
[0020] As a preferred technical solution, in step (4), the water bath temperature is 25-45°C.
[0021] The present invention also discloses a super-large straight-through pore polyethersulfone microporous filter membrane, which is prepared by the super-large straight-through pore polyethersulfone microporous filter membrane preparation method. The polyethersulfone microporous filter membrane consists of a first porous surface, a second porous surface and an intermediate connecting body. The pores of the entire filter membrane are interconnected in the longitudinal direction, and the average pore size is 1-70 μm. The pure water flux of the polyethersulfone microfiltration membrane at 0.2 MPa is 110-840 ml / cm 2 ·min.
[0022] The beneficial effects of the present invention are:
[0023] The present invention adopts a combination of high-temperature hot roller induction and steam atomization induction. On the one hand, high-temperature induction increases the activity of non-solvent molecules in the casting liquid, drives the non-solvent molecules to move quickly in the liquid film, and improves the subsequent phase separation speed of the casting liquid, which is beneficial to the construction of a through-pore structure; on the other hand, steam induction is used to control the phase separation rate of the liquid film in the induction stage, and the size of the surface pores is controlled by exchanging steam and liquid film, ultimately forming a polyethersulfone microporous filter membrane with a large pore size and a through-pore structure.
[0024] The polyethersulfone microporous filter membrane prepared by the present invention is composed of a first porous surface, a second porous surface and an intermediate connecting body. The pores of the entire filter membrane in the longitudinal direction present a mutually interpenetrating structure. The pores of the first and second porous surfaces are similar as a whole, with an average pore size of 1-70 μm. The pure water flux of the polyethersulfone microfiltration membrane at 0.2 MPa is 110-840 ml / cm 2 ·min, it has the characteristics of large pore size and high throughput compared with existing technologies. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0026] Figure 1 is a process flow chart of the present invention;
[0027] Figure 2 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 1;
[0028] Figure 3 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 1;
[0029] Figure 4 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 2;
[0030] Figure 5 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 2;
[0031] Figure 6This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 3;
[0032] Figure 7 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 3;
[0033] Figure 8 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 4;
[0034] Fig. 9 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 4;
[0035] Fig.10 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 5;
[0036] Fig.11 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 5;
[0037] Fig.12 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Comparative Example 1;
[0038] Fig.13 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Comparative Example 1;
[0039] Fig.14 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Comparative Example 2;
[0040] Fig.15 This is a cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Comparative Example 2. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0042] Example 1
[0043] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of polyethylene glycol into a stirring tank, then add 15 g of polyethersulfone and 5 g of polyvinylpyrrolidone (58,000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0044] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0045] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0046] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0047] Figure 2 This is a surface SEM photo of the polyethersulfone microporous filter membrane prepared in Example 1. Figure 3 The cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 1 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Example 1 is 1.2 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 112 ml / cm 2 ·min, the first bubble point pressure is 0.11MPa.
[0048] Example 2
[0049] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (380,000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0050] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0051] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0052] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0053] Figure 4 This is a surface SEM photo of the polyethersulfone microporous filter membrane prepared in Example 2. Figure 5 The cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 2 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Example 2 is 3 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 298 ml / cm 2·min, the first bubble point pressure is 0.06MPa.
[0054] Example 3
[0055] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0056] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0057] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0058] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0059] Figure 6 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 3. Figure 7 The cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 3 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Example 3 is 5 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 399 ml / cm 2 ·min, the first bubble point pressure is 0.038MPa.
[0060] Example 4
[0061] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0062] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0063] (3) After the liquid film was induced by a hot roller at 80°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0064] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0065] Figure 8 This is a surface SEM photo of the polyethersulfone microporous filter membrane prepared in Example 4. Fig. 9 The cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 4 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Example 4 is 10 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 490 ml / cm 2 ·min, the first bubble point pressure is 0.02MPa.
[0066] Example 5
[0067] (1) Weigh 52 g of dimethyl sulfoxide and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0068] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0069] (3) After the liquid film was induced by a hot roller at 80°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 45°C for 20 seconds.
[0070] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0071] Fig.10 This is a surface SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 5. Fig.11 The cross-sectional SEM photograph of the polyethersulfone microporous filter membrane prepared in Example 5 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Example 5 is 50 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 840 ml / cm 2 ·min, the first bubble point pressure is 0.008MPa.
[0072] Comparative Example 1
[0073] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of triethylene glycol into a stirring tank, then add 15 g of polyethersulfone and 5 g of polyvinylpyrrolidone (58000 Da) into the stirring tank, and keep the casting solution at 80°C and stir for 6 h.
[0074] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0075] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0076] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0077] Fig.12 This is a surface SEM photo of the polyethersulfone microporous filter membrane prepared in Comparative Example 1. Fig.13 The cross-sectional SEM photo of the polyethersulfone microporous filter membrane prepared in Comparative Example 1 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 1 is 0.8 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 15 ml / cm 2 ·min, the first bubble point pressure is 0.15MPa.
[0078] Comparative Example 2
[0079] (1) Weigh 60 g of N-methylpyrrolidone and 16 g of glycerol into a stirring tank, then add 15 g of polyethersulfone and 5 g of polyvinylpyrrolidone (380,000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0080] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0081] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0082] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0083] Fig.14 This is a surface SEM photo of the polyethersulfone microporous filter membrane prepared in Comparative Example 2. Fig.15 The cross-sectional SEM photo of the polyethersulfone microporous filter membrane prepared in Comparative Example 2 shows that the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 2 is 0.8 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa is 20 ml / cm 2 ·min, the first bubble point pressure is 0.135MPa.
[0084] Comparative Example 3
[0085] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of diethylene glycol dimethyl ether into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80°C and stir for 6 h.
[0086] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0087] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 85% and atomized with steam at 40°C for 20 seconds.
[0088] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0089] After testing, the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 3 was 3 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa was 50 ml / cm 2 ·min, the first bubble point pressure is 0.04MPa.
[0090] The present invention adds a specific type of additive to the casting solution, and the additive plays a pore-forming role, and also changes the aggregation state of the polymer in the solution, the thermodynamic behavior of the solution and the kinetic behavior of the gel process, thereby affecting the structure and performance of the membrane. It can be seen from Comparative Examples 1, 2 and 3 that the type of additive has a great influence on the surface pore size and performance of the polyethersulfone microporous filter membrane in the present invention.
[0091] Comparative Example 4
[0092] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (380,000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0093] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0094] (3) After the liquid film was induced by a hot roller at 60°C for 40 seconds, it was sent to a constant temperature and humidity chamber with a humidity of 50% and atomized by steam at 40°C for 20 seconds.
[0095] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0096] After testing, the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 4 was 1.2 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa was 30 ml / cm 2 ·min, the first bubble point pressure is 0.1MPa.
[0097] Comparative Example 5
[0098] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0099] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0100] (3) The liquid film was placed in a constant temperature and humidity chamber with a humidity of 50% and atomized using steam at 45°C for 20 seconds.
[0101] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0102] After testing, the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 5 was 0.45 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa was 10 ml / cm 2 ·min, the first bubble point pressure is 0.27MPa.
[0103] Comparative Example 6
[0104] (1) Weigh 52 g of N-methylpyrrolidone and 30 g of neopentyl glycol into a stirring tank, then add 15 g of polyethersulfone and 3 g of polyvinylpyrrolidone (1300000 Da) into the stirring tank, and keep the casting solution at 80° C. and stir for 6 h.
[0105] (2) After the casting liquid is stirred completely, it is poured into a pressure vessel, and after vacuuming for 0.5 h, it is placed in a constant temperature box at 80° C. The casting liquid is scraped to form a film with a film thickness of 110 μm and a pulling speed of 1 m / s to form a liquid film.
[0106] (3) The liquid film was induced by a hot roller at 80°C for 40 seconds.
[0107] (4) The liquid membrane after the induction treatment was solidified in a 30°C water bath to form a film, and then the prepared wet membrane was immersed in an aqueous solution containing 25% ethanol, the solution temperature was controlled at 30°C for cleaning, and finally the film was dried at 70°C with a drying speed of 1.5 m / s to obtain a polyethersulfone microporous filter membrane.
[0108] After testing, the surface pore size of the polyethersulfone microporous filter membrane prepared in Comparative Example 6 was 0.1 μm, and the pure water flux of the polyethersulfone microporous filter membrane at 0.2 MPa was 3 ml / cm 2 ·min, the first bubble point pressure is 0.57MPa.
[0109] The present invention adopts a combination of high-temperature hot roller induction and steam atomization induction to finally form a polyethersulfone microporous filter membrane with a large pore size and a through-pore structure. It can be seen from Comparative Examples 4, 5 and 6 that high-temperature hot roller induction and steam atomization induction and their process parameters have a great influence on the surface pore size and performance of the polyethersulfone microporous filter membrane in the present invention.
[0110] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.
Claims
1. A method for preparing a super-large straight-through-pore polyethersulfone microporous filter membrane, characterized in that: The following steps are involved: (1) dissolving polyethersulfone in a solvent, adding an additive and a porogen, and mixing them uniformly to obtain a casting solution; the additive is neopentyl glycol; the solvent is one or more of butyl lactate, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylformamide and dimethyl sulfoxide; the porogen is polyvinylpyrrolidone with a weight average molecular weight of 45000Da-1300000Da; (2) Scraping the casting liquid to form a liquid film; (3) After the liquid film is induced by a hot roller at 40-80°C for 5-60 seconds, it is sent to a constant temperature and humidity chamber with a humidity of 60-90%, and atomized by steam at 20-45°C for 5-60 seconds; (4) The liquid membrane after the induced treatment is solidified into a membrane in a water bath, and then cleaned and dried to obtain a polyethersulfone microporous filter membrane.
2. The method for preparing the ultra-large through-pore polyethersulfone microporous filter membrane according to claim 1, characterized in that: In the step (1), the mass ratio of the solvent to the polyethersulfone is 3-6:1, the mass ratio of the additive to the polyethersulfone is 0.5-3:1, and the mass ratio of the porogen to the polyethersulfone is 0.2-3:
1.
3. The method for preparing the ultra-large through-pore polyethersulfone microporous filter membrane according to claim 1, characterized in that: In the step (1), the temperature at which the polyethersulfone, solvent, additive and porogen are mixed is 50-80°C.
4. The method for preparing the ultra-large through-pore polyethersulfone microporous filter membrane according to claim 1, characterized in that: In the step (2), the scraping film thickness is 100-130 μm, and the pulling speed is 1-4 m / s.
5. The method for preparing the ultra-large through-pore polyethersulfone microporous filter membrane according to claim 1, characterized in that: In the step (4), the water bath temperature is 25-45°C.
6. A super large through-pore polyethersulfone microporous filter membrane, characterized in that: The membrane is prepared by the method for preparing a polyethersulfone microporous filter membrane with ultra-large straight through pores as described in any one of claims 1 to 5.
7. The ultra-large through-pore polyethersulfone microporous filter membrane according to claim 6, characterized in that: The polyethersulfone microporous filter membrane consists of a first porous surface, a second porous surface and an intermediate connecting body. The pores of the entire filter membrane are interconnected in the longitudinal direction, with an average pore size of 1-70μm. The pure water flux of the polyethersulfone microfiltration membrane at 0.2MPa is 110-840 ml / cm 2 ·min.