Anti-glare weather-resistant automobile head-up display film and preparation method thereof

Through the combination of modified weathering resin and coupled anti-glare micropowder, the weather resistance problem of the automotive head-up display film under high temperature and high ultraviolet rays is solved, forming a weather-resistant anti-glare layer, significantly improving the anti-glare effect and weather resistance, and solving the existing solutions The problem of yellowing in the technology.

CN118256122BActive Publication Date: 2024-11-26TIAN CHENG (SHENZHEN) MICRO-ELECTRONIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410395276.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-11-26
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

The anti-glare materials of existing automotive head-up display films have poor weather resistance and are prone to yellowing under high temperature and high ultraviolet conditions, affecting the aesthetics and projection effect. The light stabilizer in the wet process is poorly dispersed and the overall weather resistance is poor.

Method used

Using modified weathering resin and coupled anti-glare micropowder, the long-chain structure is introduced through the reaction of undecanoyl chloride and tetramethylpiperidineamine, and copolymerizes with methacrylate to form a copolymerized resin, and nanotitanium dioxide or As anti-glare particles, zinc oxide is combined with tempered glass film through a wet coating process to form a weather-resistant anti-glare layer.

Benefits of technology

It improves the weather resistance and anti-glare effect of the film layer, slows down the yellowing of polyacrylate under light and thermal conditions, enhances the adhesion and anti-glare ability of anti-glare particles, and significantly improves the weather resistance of the automotive head-up display film.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to an anti-glare weather-resistant automobile head-up display film and a preparation method thereof, belonging to the technical field of polymer film materials. The anti-glare weather-resistant automobile head-up display film is composed of a tempered glass film and a weather-resistant anti-glare layer on the surface thereof, wherein the weather-resistant anti-glare layer comprises, by weight, 100 parts of a modified weather-resistant resin, 1.1-1.7 parts of coupled anti-glare micropowder, 0.5-0.6 parts of a film-forming accelerator, 6-8 parts of an active diluent, 0.2-0.3 parts of a defoaming agent and 0.1-0.15 parts of a leveling agent; the modified weather-resistant resin is a copolymerized polyacrylate, a heterocyclic structure is introduced by a modified monomer to destroy the regularity of a copolymerized polyacrylate macromolecular chain, the mechanical toughness of a copolymerized material with methyl methacrylate as the main material is improved, a hindered amine structure is introduced at the same time, the yellowing problem of the polyacrylate under light and heat conditions is effectively slowed down, and a small amount of unsaturated structure is introduced, so that the coupled anti-glare micropowder reacts with the resin molecular chain during the curing process, the segregation of the anti-glare particles is reduced, and a good anti-glare effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer film materials, and in particular relates to an anti-glare and weather-resistant automobile head-up display film and a preparation method thereof. Background Art

[0002] Head-up display is abbreviated as HUD, also known as head-up display system, which can project the current speed, navigation and other information of the car onto the windshield, forming an image in front of the glass, so that the driver can see the navigation and speed information without turning or lowering his head. However, the traditional windshield has serious glare after projection, which affects the projection effect of the head-up display and causes visual fatigue to the driver, so anti-glare treatment is generally required.

[0003] The means for dealing with projection glare in the prior art is to form an anti-glare coating on the windshield. The coating forming methods mainly include dry method and wet method. Among them, the dry method is to deposit materials on the windshield to form a thin film through chemical vapor deposition, vacuum evaporation, sputtering, reactive ion plating and other methods to achieve the purpose of anti-glare. The products obtained by this method have good anti-glare ability and have little effect on the imaging performance of the windshield. However, this method has complex processes, strict environmental requirements for the coating process, high energy consumption and equipment costs, and low production efficiency; the wet method mainly prepares a film-forming solution through sol-gel or other methods, and then applies the film-forming solution containing anti-glare material on the surface of the substrate through spraying, spin coating, dip-pulling and other methods, and obtains the anti-glare coating after curing. Compared with the dry coating process, the process is simpler and suitable for industrial production. In the prior art, acrylate is mostly used as a wet film-forming material, which has good film-forming properties and high transparency. However, the automobile windshield is directly exposed to the sun. Under high temperature and high ultraviolet intensity, the weather resistance of the acrylate film layer is poor and it is easy to yellow, resulting in poor film imaging effect and affecting the appearance. The prior art improves the weather resistance by compounding a certain amount of light stabilizer. The added light stabilizer has poor dispersibility and is easy to segregate during the film-forming process, resulting in poor overall weather resistance. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide an anti-glare and weather-resistant automobile head-up display film and a preparation method thereof.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] An anti-glare weather-resistant automobile head-up display film is composed of a tempered glass film and a weather-resistant anti-glare layer on the surface thereof, wherein the weather-resistant anti-glare layer comprises, by weight:

[0007] 100 parts of modified weather-resistant resin, 1.1-1.7 parts of coupled anti-glare micropowder, 0.5-0.6 parts of film-forming accelerator, 6-8 parts of active diluent, 0.2-0.3 parts of defoaming agent and 0.1-0.15 parts of leveling agent.

[0008] Furthermore, the active diluent is allyl glycidyl ether.

[0009] The modified weather-resistant resin is prepared by the following method:

[0010] Step A1: tetramethylpiperidinamine, dimethylacetamide and dioxane are mixed, the temperature of the water bath is controlled at 30-40°C, mechanical stirring is applied at 120-180rpm, undecenoyl chloride is slowly added to react for 1.5-2h, and then the temperature is continued to be raised to 75-85°C, acryloyl chloride is added to continue the reaction for 30-40min, and the reaction is cooled to room temperature after the reaction is completed, water is added to wash and the water phase is removed to obtain a modified monomer;

[0011] Furthermore, the dosage ratio of tetramethylpiperidinamine, undecenoyl chloride, acryloyl chloride, dimethylacetamide and dioxane is: 0.1 mol: 0.2 mol: 0.12-0.14 mol: 8-12 mL: 65-80 mL, undecenoyl chloride preferentially reacts with the active amino group of tetramethylpiperidinamine to introduce an unsaturated olefin structure with a long-chain structure for modification, and then the highly active acryloyl chloride reacts with the residual amine structure in the substituted product to reduce the alkalinity of the product.

[0012] Step A2: Methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate and tert-butyl perbenzoate are mixed, the temperature is raised to 75-85° C., mechanical stirring is applied at 40-60 rpm, and the reaction is carried out for 35-45 minutes, and then the modified monomer is added and mixed and the reaction is continued at the temperature for 15-20 minutes. After the reaction is completed, ethyl acetate is added to dilute and the temperature is lowered to obtain a modified weather-resistant resin;

[0013] Furthermore, the usage ratio of methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate, modified monomer, tert-butyl perbenzoate and ethyl acetate is 0.1 mol: 15-30 mmol: 25-40 mmol: 20-30 mmol: 0.15-0.2 g: 10-15 mL, and methyl methacrylate is used as a base material, which is first copolymerized with the remaining acrylates to form an oligomer, and then repolymerized with the modified monomer to form a copolymer resin.

[0014] The preparation method of the coupled anti-glare micropowder is as follows: silane coupling agent KH-580 and oxygen-free ethanol solution are mixed under nitrogen protection, the pH value is adjusted to 5 with hydrochloric acid, stirred and hydrolyzed for 40-50 minutes, and then nano anti-glare filler is added for ultrasonic dispersion, neutralized with ammonia water, allowed to stand for 12 hours, centrifuged to remove the supernatant, and vacuum dried to obtain the coupled anti-glare micropowder.

[0015] Furthermore, the nano anti-glare filler is one of nano titanium dioxide and nano zinc oxide, or a mixture of the two in any proportion.

[0016] Furthermore, the usage ratio of the nano anti-glare filler, the silane coupling agent KH-580 and the oxygen-free ethanol solution is 100 g: 1.5-2.2 g: 280-350 mL, and the mass fraction of the oxygen-free ethanol solution is 30-40%.

[0017] A method for preparing an anti-glare weather-resistant automobile head-up display film comprises the following steps:

[0018] Step S1: premixing the coupled anti-glare micropowder, active diluent, defoamer and leveling agent, adding the modified weather-resistant resin and film-forming accelerator, mixing evenly, and vacuum degassing to obtain an anti-glare coating;

[0019] Step S2: Wipe the surface of the tempered glass film with ethanol and dry it, then scrape the anti-glare coating on the surface, place it in a UV curing furnace for drying and curing after leveling, and form a weather-resistant anti-glare layer on the surface of the tempered glass film, so as to obtain an anti-glare and weather-resistant automotive head-up display film.

[0020] Furthermore, the parameters in the UV curing oven are set as follows: the temperature of zone 1 is 60-70°C, 180-240W / m 2 UV irradiation, time is 150-240s; temperature in zone 2 is 50-55℃, 120-160W / m 2 Ultraviolet irradiation, time is 180-300s; the temperature of the third zone is 40-50℃, no irradiation, time is 300-400s.

[0021] Beneficial effects of the present invention:

[0022] The invention adopts a wet coating process and a tempered glass film to produce an anti-glare film in combination. The process is simple and the quality is controllable. The film layer uses a modified weather-resistant resin as a film-forming material and uses coupled titanium dioxide or zinc oxide as anti-glare particles. The modified weather-resistant resin is modified by preferentially reacting undecylenyl chloride with the active amino group of tetramethylpiperidinamine to introduce an unsaturated olefin structure with a long-chain structure. Then, highly active acryloyl chloride reacts with the residual amine structure in the substitution product to prepare a modified monomer, which is then copolymerized with methyl methacrylate, ethyl acrylate and hydroxyethyl methacrylate to form a copolymerized polyacrylate. The heterocyclic structure in the modified monomer destroys the regularity of the copolymerized polyacrylate macromolecular chain and improves the mechanical toughness of the copolymerized material with methyl methacrylate as the main material. At the same time, a hindered amine structure is uniformly introduced into the film layer through copolymerization, which effectively slows down the yellowing problem of the polyacrylate under light and heat conditions. In addition, a small amount of unsaturated structure is introduced into the resin through copolymerization of the modified monomer, so that the coupled anti-glare micropowder reacts with the resin molecular chain during the curing process, reduces the segregation of the anti-glare particles, and achieves a good anti-glare effect. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Specific implementation method 1, preparing an anti-glare weather-resistant automobile head-up display film, specifically as follows:

[0025] 1) Preparation of modified weather-resistant resin

[0026] Step A1: Take tetramethylpiperidinamine, dimethylacetamide and dioxane and mix them evenly, control the temperature of the water bath to 40°C, apply mechanical stirring at 180rpm, slowly add undecylenyl chloride to react for 1.5h, then continue to heat to 85°C, add acryloyl chloride and continue to react for 30min. During the reaction, the amount ratio of tetramethylpiperidinamine, undecylenyl chloride, acryloyl chloride, dimethylacetamide and dioxane is: 0.1mol: 0.2mol: 0.14mol: 8mL: 80mL. After the reaction is completed, cool to room temperature, add water to wash and remove the aqueous phase to obtain a modified monomer.

[0027] Step A2: Take methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate and tert-butyl perbenzoate, mix them, heat to 85°C, apply mechanical stirring at 60rpm, react for 35 minutes, then add modified monomer, mix and continue to keep warm for 15 minutes. After the reaction is completed, add ethyl acetate to dilute and cool down. During the reaction, the amount ratio of methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate, modified monomer, tert-butyl perbenzoate and ethyl acetate is 0.1mol:30mmol:25mmol:30mmol:0.15g:15mL to obtain a modified weather-resistant resin.

[0028] 2) Preparation of coupled anti-glare micropowder

[0029] Prepare a 30% mass fraction of oxygen-free ethanol solution, take silane coupling agent KH-580 and oxygen-free ethanol solution, mix them under nitrogen protection, adjust the pH value to 5 with hydrochloric acid, stir and hydrolyze for 40 minutes, and then add nano anti-glare filler. In this implementation method, JWN-R15 nano titanium dioxide provided by Ningbo Jiwei Nano New Material Technology Co., Ltd. is used. It is ultrasonically dispersed at 25kHz for 10 minutes, then added with ammonia water for neutralization, and allowed to stand for 12 hours. During the reaction, the amount ratio of nano anti-glare filler, silane coupling agent KH-580 and oxygen-free ethanol solution is 100g:1.5g:280mL. Then, the supernatant is removed by centrifugation and vacuum dried to obtain coupled anti-glare micropowder.

[0030] 3) Preparation of composite membrane materials

[0031] The raw materials are taken according to weight parts: 100 parts of modified weather-resistant resin, prepared by this embodiment; 1.1 parts of coupled anti-glare micropowder, prepared by this embodiment; 0.5 parts of film-forming promoter, J2502 type raw material is used in the implementation process, and drying promotes film formation; 6 parts of active diluent, allyl glycidyl ether, industrial grade raw material is used in the implementation process; 0.3 parts of defoaming agent, BYK-088 type raw material is used in the implementation process; 0.1 parts of leveling agent, BYK-371 type raw material is used in the implementation process.

[0032] Step S1: Add coupled anti-glare micropowder, active diluent, defoamer and leveling agent, premix at 600 rpm for 5 min, then add modified weather-resistant resin and film-forming accelerator, stir at 120 rpm for 10 min, and vacuum degas to obtain anti-glare coating.

[0033] Step S2: Take a tempered glass film (all commercially available 0.2 mm optical tempered glass), wipe the surface with ethanol and dry it, then apply anti-glare coating on the surface, let it level naturally for 30 minutes, and place it in a UV curing furnace. The parameters in the control furnace are set as follows: the temperature of zone 1 is 70°C, 240W / m 2 UV irradiation, time is 150s; temperature of zone 2 is 55℃, 160W / m 2 Ultraviolet irradiation for 180 seconds; the temperature of the third zone is 50°C, no irradiation for 300 seconds, the anti-glare coating is cured on the surface of the tempered glass film to form a weather-resistant anti-glare layer to make a head-up display film.

[0034] Specific embodiment 2, preparing an anti-glare weather-resistant automobile head-up display film, specifically as follows:

[0035] 1) Preparation of modified weather-resistant resin

[0036] Step A1: Take tetramethylpiperidinamine, dimethylacetamide and dioxane and mix them evenly, control the temperature of the water bath to 30°C, apply mechanical stirring at 120rpm, slowly add undecylenyl chloride to react for 2h, then continue to heat to 75°C, add acryloyl chloride and continue to react for 40min. During the reaction, the amount ratio of tetramethylpiperidinamine, undecylenyl chloride, acryloyl chloride, dimethylacetamide and dioxane is: 0.1mol: 0.2mol: 0.12mol: 12mL: 65mL. After the reaction is completed, cool to room temperature, add water to wash and remove the aqueous phase to obtain a modified monomer.

[0037] Step A2: Take methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate and tert-butyl perbenzoate, mix them, heat to 75°C, apply mechanical stirring at 40rpm, react for 45 minutes, then add modified monomer, mix and continue to keep warm for 20 minutes. After the reaction is completed, add ethyl acetate to dilute and cool down. During the reaction, the amount ratio of methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate, modified monomer, tert-butyl perbenzoate and ethyl acetate is 0.1 mol: 15 mmol: 40 mmol: 20 mmol: 0.2 g: 10 mL to obtain a modified weather-resistant resin.

[0038] 2) Preparation of coupled anti-glare micropowder

[0039] Prepare a 40% mass fraction of anaerobic ethanol solution, take silane coupling agent KH-580 and anaerobic ethanol solution, mix them under nitrogen protection, adjust the pH value to 5 with hydrochloric acid, stir and hydrolyze for 50 minutes, and then add nano anti-glare filler. In this implementation method, ZT-AZO nano zinc oxide provided by Zhejiang Zhiti Nano Micro New Materials Co., Ltd. is used, ultrasonically dispersed at 25kHz for 10 minutes, then added with ammonia water for neutralization, and allowed to stand for 12 hours. During the reaction, the amount ratio of nano anti-glare filler, silane coupling agent KH-580 and anaerobic ethanol solution is 100g:2.2g:350mL, then centrifuged to remove the supernatant, and vacuum dried to obtain coupled anti-glare micropowder.

[0040] 3) Preparation of composite membrane materials

[0041] The raw materials are taken in parts by weight: 100 parts of modified weather-resistant resin, prepared in this example; 1.7 parts of coupled anti-glare micropowder, prepared in this example; 0.5 parts of film-forming accelerator, 8 parts of active diluent, 0.2 parts of defoaming agent and 0.15 parts of leveling agent.

[0042] Step S1: Add coupled anti-glare micropowder, active diluent, defoamer and leveling agent, premix at 600 rpm for 5 min, then add modified weather-resistant resin and film-forming accelerator, stir at 120 rpm for 10 min, and vacuum degas to obtain anti-glare coating.

[0043] Step S2: Take the tempered glass film, wipe the surface with ethanol and dry it, then apply anti-glare coating on the surface, let it level naturally for 30 minutes, and place it in a UV curing furnace. The control parameters in the furnace are set as follows: the temperature of zone 1 is 60℃, 180W / m 2 UV irradiation, time is 240s; temperature of zone 2 is 50℃, 120W / m 2 UV irradiation for 300s; the temperature of the third zone is 40℃, no irradiation for 400s, the anti-glare coating is cured on the surface of the tempered glass film to form a weather-resistant anti-glare layer to make a head-up display film.

[0044] Specific implementation method 3, preparing an anti-glare weather-resistant automotive head-up display film, specifically as follows:

[0045] 1) Preparation of modified weather-resistant resin

[0046] Step A1: Take tetramethylpiperidinamine, dimethylacetamide and dioxane and mix them evenly. The temperature of the water bath is controlled at 35°C. Mechanical stirring is applied at 180rpm. Undecenoyl chloride is slowly added to react for 1.8h. Then the temperature is continued to rise to 82°C. Acryloyl chloride is added to continue the reaction for 35min. During the reaction, the amount ratio of tetramethylpiperidinamine, undecenoyl chloride, acryloyl chloride, dimethylacetamide and dioxane is: 0.1mol: 0.2mol: 0.13mol: 10mL: 75mL. After the reaction is completed, cool to room temperature, add water for washing and remove the aqueous phase to obtain a modified monomer.

[0047] Step A2: Take methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate and tert-butyl perbenzoate, mix them, heat to 80°C, apply mechanical stirring at 60rpm, react for 40 minutes, then add the modified monomer, mix and continue to keep warm for 18 minutes. After the reaction is completed, add ethyl acetate to dilute and cool down. During the reaction, the amount ratio of methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate, modified monomer, tert-butyl perbenzoate and ethyl acetate is 0.1 mol: 25 mmol: 30 mmol: 25 mmol: 0.18 g: 12 mL to obtain a modified weather-resistant resin.

[0048] 2) Preparation of coupled anti-glare micropowder

[0049] Prepare a 30% mass fraction of oxygen-free ethanol solution, take silane coupling agent KH-580 and oxygen-free ethanol solution, mix them under nitrogen protection, adjust the pH value to 5 with hydrochloric acid, stir and hydrolyze for 50 minutes, and then add nano anti-glare filler. In this implementation method, JWN-R15 nano titanium dioxide and ZT-AZO nano zinc oxide are mixed in a mass ratio of 1:1; ultrasonic dispersion is carried out at 25kHz for 10 minutes, and then ammonia water is added for neutralization, and the mixture is allowed to stand for 12 hours. During the reaction, the amount ratio of nano anti-glare filler, silane coupling agent KH-580 and oxygen-free ethanol solution is 100g:1.9g:320mL, and then the supernatant is removed by centrifugation and vacuum drying is obtained to obtain coupled anti-glare micropowder.

[0050] 3) Preparation of composite membrane materials

[0051] The raw materials are taken in parts by weight: 100 parts of modified weather-resistant resin, prepared in this example; 1.4 parts of coupled anti-glare micropowder, prepared in this example; 0.6 parts of film-forming accelerator, 7 parts of active diluent, 0.2 parts of defoaming agent and 0.13 parts of leveling agent.

[0052] Step S1: Add coupled anti-glare micropowder, active diluent, defoamer and leveling agent, premix at 600 rpm for 5 min, then add modified weather-resistant resin and film-forming accelerator, stir at 120 rpm for 10 min, and vacuum degas to obtain anti-glare coating.

[0053] Step S2: Take the tempered glass film, wipe the surface with ethanol and dry it, then apply anti-glare coating on the surface, let it level naturally for 30 minutes, put it in a UV curing furnace, and control the parameters in the furnace to set: the temperature of zone 1 is 65℃, 220W / m 2 UV irradiation, time is 200s; temperature of zone 2 is 55℃, 140W / m 2 UV irradiation for 260s; the temperature of the third zone is 50℃, no irradiation for 350s, the anti-glare coating is cured on the surface of the tempered glass film to form a weather-resistant anti-glare layer to make a head-up display film.

[0054] Comparative Example

[0055] This comparative example refers to Example 3, except that no modified monomer is added in step A2 of preparing the modified weather-resistant resin, 0.08 parts of light stabilizer GW-508 is added to the raw materials for preparing the composite film material, and the rest are exactly the same.

[0056] Samples were taken from the above-prepared film materials to test the anti-glare performance of the film materials, including transmittance, haze and 60° glossiness tests. The specific test data are shown in Table 1:

[0057] Table 1

[0058] Light transmittance / % Haze / % 60° gloss / % Example 1 94.1 7.39 76.3 Example 2 90.8 8.64 71.5 Example 3 93.4 8.05 74.2 Comparative Example 91.2 6.42 82.7

[0059] It can be seen from the data in Table 1 that the light transmittance, haze and 60° glossiness of the films prepared in the examples and comparative examples are all within a good range of values ​​and have good anti-glare capabilities.

[0060] Samples were taken from the prepared film materials to test the performance of the film materials, including the adhesion test of the weather-resistant and anti-glare layer, the impact test and the weather resistance test. The weather resistance test was a light-heat yellowing test. The specific method was as follows: the sample was placed in a UV oven, the temperature was controlled at 60°C, and the UV radiation intensity was 120W / m 2 , treated for 720h, simulated outdoor exposure environment, and used a spectrophotometer to measure the color difference before and after treatment. The specific test data are shown in Table 2:

[0061] Table 2

[0062] Adhesion / Grade Impact strength / cm Light and thermal color difference Example 1 0 50 0.14 Example 2 0 50 0.22 Example 3 0 50 0.17 Comparative Example 0 40 0.85

[0063] It can be seen from the data in Table 2 that the weather-resistant anti-glare layer of the film material prepared in the embodiment has good adhesion, high impact strength, low light and heat color difference, and exhibits excellent weather resistance.

[0064] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0065] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An anti-glare weather-resistant automobile head-up display film, consisting of a tempered glass film and a weather-resistant anti-glare layer on its surface, characterized in that: The weather-resistant and anti-glare layer comprises, by weight: 100 parts of modified weather-resistant resin, 1.1-1.7 parts of coupled anti-glare micropowder, 0.5-0.6 parts of film-forming accelerator, 6-8 parts of active diluent, 0.2-0.3 parts of defoamer and 0.1-0.15 parts of leveling agent; The modified weather-resistant resin is prepared by the following method: Step A1: tetramethylpiperidinamine, dimethylacetamide and dioxane are mixed, the temperature of the water bath is controlled at 30-40°C, undecenoyl chloride is slowly added with stirring to react for 1.5-2h, then the temperature is continued to be raised to 75-85°C, acryloyl chloride is added to continue the reaction for 30-40min, after the reaction is completed, the mixture is cooled to room temperature, water is added to wash and the aqueous phase is removed to obtain a modified monomer; Step A2: Methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate and tert-butyl perbenzoate are mixed, heated to 75-85°C, stirred and reacted for 35-45 minutes, then modified monomers are added and mixed and the reaction is continued at the temperature for 15-20 minutes. After the reaction is completed, ethyl acetate is added to dilute and the temperature is lowered to obtain a modified weather-resistant resin.

2. The anti-glare weather-resistant automotive head-up display film according to claim 1, characterized in that: The usage ratio of tetramethylpiperidinamine, undecenoyl chloride, acryloyl chloride, dimethylacetamide and dioxane is: 0.1 mol: 0.2 mol: 0.12-0.14 mol: 8-12 mL: 65-80 mL.

3. The anti-glare weather-resistant automotive head-up display film according to claim 2, characterized in that: The usage ratio of methyl methacrylate, ethyl acrylate, hydroxyethyl methacrylate, modified monomer, tert-butyl perbenzoate and ethyl acetate is 0.1 mol: 15-30 mmol: 25-40 mmol: 20-30 mmol: 0.15-0.2 g: 10-15 mL.

4. The anti-glare weather-resistant automotive head-up display film according to claim 1, characterized in that: The preparation method of the coupled anti-glare micropowder is as follows: silane coupling agent KH-580 and oxygen-free ethanol solution are mixed under nitrogen protection, the pH value is adjusted to 5 with hydrochloric acid, stirred and hydrolyzed for 40-50 minutes, and then nano anti-glare filler is added for ultrasonic dispersion, neutralized with ammonia water, allowed to stand for 12 hours, centrifuged to remove the supernatant, and vacuum dried to obtain the coupled anti-glare micropowder.

5. The anti-glare weather-resistant automotive head-up display film according to claim 4, characterized in that: The nano anti-glare filler is one of nano titanium dioxide and nano zinc oxide or a mixture of the two in any proportion.

6. The anti-glare weather-resistant automotive head-up display film according to claim 5, characterized in that: The dosage ratio of the nano anti-glare filler, the silane coupling agent KH-580 and the oxygen-free ethanol solution is 100g: 1.5-2.2g: 280-350mL, and the mass fraction of the oxygen-free ethanol solution is 30-40%.

7. The method for preparing an anti-glare weather-resistant automobile head-up display film according to claim 1, characterized in that: The steps include: Step S1: premixing the coupled anti-glare micropowder, active diluent, defoamer and leveling agent, adding the modified weather-resistant resin and film-forming accelerator, mixing evenly, and vacuum degassing to obtain an anti-glare coating; Step S2: Wipe the surface of the tempered glass film with ethanol and dry it, then apply anti-glare coating on the surface, place it in a UV curing oven for drying and curing after leveling, and form a weather-resistant anti-glare layer on the surface of the tempered glass film, so as to obtain an anti-glare and weather-resistant automotive head-up display film.

8. The method for preparing an anti-glare weather-resistant automobile head-up display film according to claim 7, characterized in that: The parameters in the UV curing oven are set as follows: Zone 1 temperature is 60-70°C, 180-240W / m 2 UV irradiation, time is 150-240s; temperature in zone 2 is 50-55℃, 120-160W / m 2 Ultraviolet irradiation, time is 180-300s; the temperature of the third zone is 40-50℃, no irradiation, time is 300-400s.