A composite containing silicone release agent and pressure-sensitive adhesive
By using hydrogen silicon addition cured polysiloxane release agent on pressure-sensitive adhesive paper to form an excellent release layer, the problem of insufficient release of pressure-sensitive adhesive paper is solved, and efficient adhesion and peeling performance are achieved. To ensure that the product does not deform under external force, it improves the stability and practicality of use.
Patent Information
- Application Number
- CN202410469936.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-04-18
AI Technical Summary
The release properties of existing pressure-sensitive adhesive papers are poor and are prone to deform when pulled by external forces, which will affect their use.
Using a composite containing silicone release agent, an excellent release layer is formed by coating and curing, and combined with a pressure-sensitive adhesive layer, the integration of pressure-sensitive and peeling effects is achieved. This release agent is a hydrosilica-addition cured polysiloxane release agent, which has low surface free energy and flexibility, prevents adhesion and deformation, and is easy to rebound and restore when pulled by external force.
It realizes excellent peeling force and softness of pressure-sensitive adhesive paper, ensuring that the pressure-sensitive layer is not contaminated before sticking, does not lose its viscosity after use, and is not easy to deform under external forces, improving the practicality and stability of the product.
Smart Images

Figure BDA0004798617550000111 
Figure BDA0004798617550000121 
Figure BDA0004798617550000122
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of integrated release agent and pressure-sensitive adhesive, and in particular relates to a composite body containing an organic silicon release agent and a pressure-sensitive adhesive. Background Art
[0002] Release pressure-sensitive composite is a kind of pressure-sensitive adhesive paper (or cloth) tape, which is commonly used in adhesive applications in various industries. Pressure-sensitive adhesive tape is usually designed like transparent tape with one side sticky and the other side not sticky. The sticky side is a pressure-sensitive adhesive layer, which is rolled up tightly on the non-sticky release layer. This design can prevent the pressure-sensitive adhesive tape from sticking to each other and deforming, and can protect the pressure-sensitive layer from being contaminated before being pasted and used, which is convenient for storage and sale, and more convenient for subsequent practical use. Pressure-sensitive adhesive tape is widely used in medical, office and home fields. In the medical field, pressure-sensitive adhesive tape is mainly used to fix bandages, fix catheters and pipes, cover wounds, protect skin, etc.; in the office field, pressure-sensitive adhesive tape is mainly used to paste paper, seal envelopes, repair documents, mark items, etc.; in home life, pressure-sensitive adhesive tape is mainly used to fix some small items to prevent them from loosening or falling off.
[0003] The main feature of pressure-sensitive adhesive tape is that it can be adhered to various surfaces with just a little pressure, and can be peeled off and re-adhered at any time. This requires that the pressure-sensitive layer of the pressure-sensitive adhesive tape has excellent adhesion, and the release layer needs to have excellent release properties and drive the entire pressure-sensitive adhesive tape to rebound and recover easily without deformation when pulled by external force, otherwise it will easily affect the use. Therefore, it is particularly necessary to provide a pressure-sensitive adhesive tape with excellent release properties and not easy to deform when pulled by external force. Summary of the invention
[0004] The object of the present invention is to provide a composite body containing an organic silicone release agent and a pressure-sensitive adhesive, wherein the composite body comprises a release layer, a substrate layer and a pressure-sensitive layer; the release layer is obtained by coating and curing the release agent; the release agent is any one of a hydrosilylation-cured polysiloxane release agent, a condensation-cured polysiloxane release agent, a peroxide-cured polysiloxane release agent, and a light-cured polysiloxane release agent. The release layer in the composite body prepared by the present invention has good peeling force, and the composite body has excellent release performance and is easy to rebound and recover without deformation when pulled by external force, which solves the problems of poor release of pressure-sensitive adhesive paper and easy deformation when pulled by external force in the prior art.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A composite body containing an organic silicon release agent and a pressure-sensitive adhesive, the composite body comprising a release layer, a substrate layer and a pressure-sensitive layer; the release layer is located on one side of the substrate layer, and the pressure-sensitive layer is located on the other side of the substrate layer;
[0007] The release layer is obtained by coating and curing a release agent, and the release agent is any one of a silylation-curing polysiloxane release agent, a condensation-curing polysiloxane release agent, a peroxide-curing polysiloxane release agent, and a light-curing polysiloxane release agent; the pressure-sensitive layer is obtained by coating and curing a pressure-sensitive adhesive; the substrate layer is any one of cotton cloth, glass cloth, non-woven fabric, PS, kraft paper, glassine paper, and coated paper.
[0008] The release layer of the present invention has low surface free energy and good softness, which can prevent the pressure-sensitive adhesive tape from sticking to each other and deforming, and is convenient for winding; the pressure-sensitive layer is very sensitive to pressure and can immediately achieve a bonding effect on the adherend under a relatively small pressure; the pressure-sensitive adhesive tape containing the silicone release agent prepared by the present invention realizes the integration of pressure sensitivity and peeling effect, and has excellent practicality.
[0009] As a preferred technical solution of the present invention, the preparation process of the composite comprises the following steps:
[0010] A1. Clean, wind and move the substrate layer forward: clean the pollutants on the surface of the substrate layer, wind the cleaned substrate layer on the driving roller of the coating machine, and drive the substrate layer forward with the driving roller;
[0011] A2. Applying a release agent and a pressure-sensitive adhesive to the substrate layer: applying a release agent to one side of the substrate layer and curing it, and then applying a pressure-sensitive adhesive to the other side of the substrate layer and curing it;
[0012] A3. Winding: The substrate layer coated with the release agent and the pressure-sensitive adhesive is wound up by a winding roller to obtain a composite.
[0013] As a preferred technical solution of the present invention, the pressure-sensitive adhesive is a silicone pressure-sensitive adhesive, and the brand is Wanhua Chemical SA1511.
[0014] As a preferred technical solution of the present invention, the release agent and the pressure-sensitive adhesive are coated with a thickness of 5-10 μm.
[0015] As a preferred technical solution of the present invention, the preparation method of the hydrosilylation type polysiloxane release agent specifically comprises the following steps:
[0016] S1. Evenly mix the epoxy-terminated silicone oil, ED-900 polyetheramine and isopropanol, control the temperature for reaction, maintain the temperature, and then add 2,3-epoxypropyltrimethylammonium chloride for reaction to obtain intermediate material A for standby use;
[0017] S2, controlling the temperature and stirring the vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and catalyst to obtain intermediate material B for later use;
[0018] S3. In a nitrogen atmosphere, the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and the catalyst are stirred under controlled temperature, and the temperature is maintained. The intermediate material B is added to react to obtain the release agent.
[0019] As a preferred technical solution of the present invention, the mass ratio of the epoxy-terminated silicone oil, ED-900 polyetheramine, isopropanol and 2,3-epoxypropyltrimethylammonium chloride in step S1 is 18-23:1.65-2.15:20-26:0.55-0.72.
[0020] As a preferred technical solution of the present invention, the temperature of the temperature-controlled reaction in step S1 is 80-85° C., and the reaction time is 3-3.5 h; the reaction time of adding 2,3-epoxypropyltrimethylammonium chloride is 2.5-3 h.
[0021] As a preferred technical solution of the present invention, the viscosity of the vinyl-terminated silicone oil in step S2 is 500-1000cp.
[0022] As a preferred technical solution of the present invention, the hydrogen-containing silicone oil in step S2 includes hydrogen-containing silicone oil with a hydrogen content of 1.6% and hydrogen-containing silicone oil with a hydrogen content of 0.75%.
[0023] As a preferred technical solution of the present invention, the mass ratio of the hydrogen-containing silicone oil with a hydrogen content of 1.6% to the hydrogen-containing silicone oil with a hydrogen content of 0.75% is 2:3.
[0024] As a preferred technical solution of the present invention, the mass ratio of the vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and catalyst in step S2 is 25-30:46-52:10-12:1.2-1.6:1-1.3.
[0025] As a preferred technical solution of the present invention, the stabilizer in step S2 includes SLS, OP-10 and SLS.
[0026] As a preferred technical solution of the present invention, the mass ratio of the Methyl 45, OP-10 and SLS is 1:2-2.5:0.5.
[0027] As a preferred technical solution of the present invention, the catalyst is a Karstedt catalyst.
[0028] As a preferred technical solution of the present invention, the temperature for temperature-controlled stirring in step S2 is 60-65°C.
[0029] As a preferred technical solution of the present invention, the mass ratio of the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, catalyst and intermediate material B in step S3 is 1:0.3-0.4:0.06-0.07:1.
[0030] As a preferred technical solution of the present invention, the catalyst is trifluoromethanesulfonic acid.
[0031] As a preferred technical solution of the present invention, the temperature of the temperature-controlled stirring in step S3 is 70-75°C and the time is 3-4h; the reaction time of the reaction is 1-2h.
[0032] Beneficial effects of the present invention:
[0033] (1) The present invention uses epoxy-terminated silicone oil and vinyl-terminated silicone oil at the same time, and mixes two hydrogen-containing silicone oils with different hydrogen contents. Long and short chains are interlaced with each other, which is conducive to forming a dense network structure. At the same time, the present invention reacts ED-900 polyetheramine and epoxy-terminated silicone oil to make the system contain silicon-oxygen bonds with large bond energy and bond angle and low surface free energy. On this basis, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane is introduced to provide fluorine-containing groups, which strongly reduces the surface free energy of the system, so that the prepared release layer has good peeling force; the release agent is used in the preparation of the release layer of pressure-sensitive adhesive paper, which also gives the pressure-sensitive adhesive paper excellent peeling performance, so that the release layer of the finished pressure-sensitive adhesive paper can protect the pressure-sensitive layer, so that the pressure-sensitive layer will not be contaminated before being pasted and used, and will not lose its viscosity.
[0034] (2) The present invention adds ED-900 polyetheramine and epoxy-terminated silicone oil to react with each other. The polysiloxane chain segments with a helical structure in the system give the release agent excellent softness and resilience. On this basis, 2,3-epoxypropyltrimethylammonium chloride is added to introduce a quaternary ammonium salt, which improves the bonding force between the release agent and the substrate and makes the release agent adhere to the surface of the substrate more regularly, further enhancing the softness of the release agent. Therefore, the prepared release agent is coated on the substrate so that the final pressure-sensitive adhesive tape product can easily rebound and recover without deformation when being pulled by external force.
[0035] (3) The present invention compounds SLS with 45, OP-10 and SLS to form an anionic-nonionic system, which can synergistically make the prepared release agent less likely to demulsify, float oil or stratify, and has excellent storage stability and centrifugal stability, thereby ensuring the use quality of the release agent. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] A composite body containing an organic silicon release agent and a pressure-sensitive adhesive, wherein the composite body is composed of a release layer, a substrate layer and a pressure-sensitive layer from bottom to top; the release layer is obtained by coating and curing a silicon hydrogen addition type polysiloxane release agent; the pressure-sensitive layer is obtained by coating and curing a pressure-sensitive adhesive;
[0039] The substrate layer is glass cloth;
[0040] The pressure-sensitive adhesive is an organic silicon pressure-sensitive adhesive with the brand name of Wanhua Chemical SA1511;
[0041] The release agent coating thickness is 5 μm, and the pressure-sensitive adhesive coating thickness is 7 μm;
[0042] The preparation process of the composite comprises the following steps:
[0043] A1. Clean, wind and move the glass cloth forward: clean the pollutants on the surface of the glass cloth, wind the cleaned glass cloth on the driving roller of the coating machine, and use the driving roller to drive the glass cloth forward;
[0044] A2. Apply release agent and pressure-sensitive adhesive to the glass cloth: Apply silicon hydrogen addition type polysiloxane release agent to one side of the glass cloth, and then cure it. Then apply Wanhua Chemical SA1511 silicone pressure-sensitive adhesive to the other side of the glass cloth, and then harden it.
[0045] A3. Winding: The glass cloth coated with release agent and pressure-sensitive adhesive is rolled up by a winding roller to form a composite.
[0046] The method for preparing the hydrosilylation type polysiloxane release agent in step A2 specifically comprises the following steps:
[0047] S1. Evenly mix the epoxy-terminated silicone oil, ED-900 polyetheramine and isopropanol, control the temperature to 80°C for reaction for 3 hours, maintain the temperature at 85°C, add 2,3-epoxypropyltrimethylammonium chloride and react for 2.5 hours to obtain intermediate material A for standby use;
[0048] The mass ratio of the epoxy-terminated silicone oil, ED-900 polyetheramine, isopropyl alcohol and 2,3-epoxypropyltrimethylammonium chloride is 18:1.9:20:0.72;
[0049] S2, vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and Karstedt catalyst are mixed at a mass ratio of 30:46:10:1.4:1 at 60°C to obtain intermediate material B for standby use;
[0050] The viscosity of the vinyl-terminated silicone oil is 500cp;
[0051] The hydrogen-containing silicone oil comprises hydrogen-containing silicone oil with a hydrogen content of 1.6% and hydrogen-containing silicone oil with a hydrogen content of 0.75% in a mass ratio of 2:3;
[0052] The stabilizer comprises SLS, OP-10 and SLS in a mass ratio of 1:2.5:0.5;
[0053] S3. In a nitrogen atmosphere, the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and trifluoromethanesulfonic acid were stirred at 75° C. for 3 h, the temperature was maintained at 70° C., and the intermediate material B was added and reacted for 1 h to obtain a release agent;
[0054] The mass ratio of the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, trifluoromethanesulfonic acid and the intermediate material B is 1:0.35:0.06:1.
[0055] Example 2
[0056] A composite body containing an organic silicon release agent and a pressure-sensitive adhesive, wherein the composite body is composed of a release layer, a substrate layer and a pressure-sensitive layer from bottom to top; the release layer is obtained by coating and curing a silicon hydrogen addition type polysiloxane release agent; the pressure-sensitive layer is obtained by coating and curing a pressure-sensitive adhesive;
[0057] The substrate layer is a non-woven fabric;
[0058] The pressure-sensitive adhesive is an organic silicon pressure-sensitive adhesive with the brand name of Wanhua Chemical SA1511;
[0059] The release agent coating thickness is 7 μm, and the pressure-sensitive adhesive coating thickness is 5 μm;
[0060] The preparation process of the composite comprises the following steps:
[0061] A1. Clean, wind and move the non-woven fabric forward: clean the pollutants on the surface of the non-woven fabric, wind the cleaned non-woven fabric on the driving roller of the coating machine, and use the driving roller to drive the non-woven fabric forward;
[0062] A2. Apply release agent and pressure-sensitive adhesive to the non-woven fabric: Apply a silicon-hydrogen addition type polysiloxane release agent to one side of the non-woven fabric, and then cure it. Then apply Wanhua Chemical SA1511 silicone pressure-sensitive adhesive to the other side of the non-woven fabric, and then cure it.
[0063] A3. Winding: The nonwoven fabric coated with the release agent and the pressure-sensitive adhesive is rolled up by a winding roller to obtain a composite.
[0064] The method for preparing the hydrosilylation type polysiloxane release agent in step A2 specifically comprises the following steps:
[0065] S1. Evenly mix the epoxy-terminated silicone oil, ED-900 polyetheramine and isopropanol, control the temperature to 85°C for reaction for 3 hours, maintain the temperature at 83°C, then add 2,3-epoxypropyltrimethylammonium chloride and react for 3 hours to obtain intermediate material A for standby use;
[0066] The mass ratio of the epoxy-terminated silicone oil, ED-900 polyetheramine, isopropyl alcohol and 2,3-epoxypropyltrimethylammonium chloride is 23:1.65:26:0.55;
[0067] S2, vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and Karstedt catalyst are mixed at a mass ratio of 25:52:11:1.26:1.3 at 65°C to obtain intermediate material B for standby use;
[0068] The viscosity of the vinyl-terminated silicone oil is 750cp;
[0069] The hydrogen-containing silicone oil comprises hydrogen-containing silicone oil with a hydrogen content of 1.6% and hydrogen-containing silicone oil with a hydrogen content of 0.75% in a mass ratio of 2:3;
[0070] The stabilizer comprises SLS, OP-10 and SLS in a mass ratio of 1:2:0.5;
[0071] S3. In a nitrogen atmosphere, the intermediate material A, 1,3,5-trimethyl-1,3,5-tri(3,3,3-trifluoropropyl)cyclotrisiloxane and trifluoromethanesulfonic acid were stirred at 73° C. for 3.5 hours, and the temperature was maintained at 73° C. The intermediate material B was added and reacted for 1.5 hours to obtain a release agent;
[0072] The mass ratio of the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, trifluoromethanesulfonic acid and the intermediate material B is 1:0.4:0.065:1.
[0073] Example 3
[0074] A composite body containing an organic silicon release agent and a pressure-sensitive adhesive, wherein the composite body is composed of a release layer, a substrate layer and a pressure-sensitive layer from bottom to top; the release layer is obtained by coating and curing a silicon hydrogen addition type polysiloxane release agent; the pressure-sensitive layer is obtained by coating and curing a pressure-sensitive adhesive;
[0075] The substrate layer is kraft paper;
[0076] The pressure-sensitive adhesive is an organic silicon pressure-sensitive adhesive with the brand name of Wanhua Chemical SA1511;
[0077] The release agent coating thickness is 10 μm, and the pressure-sensitive adhesive coating thickness is 10 μm;
[0078] The preparation process of the composite comprises the following steps:
[0079] A1. Clean, roll and run the kraft paper forward: clean the pollutants on the surface of the kraft paper, roll the cleaned kraft paper on the driving roller of the coating machine, and use the driving roller to drive the kraft paper forward;
[0080] A2. Apply release agent and pressure-sensitive adhesive to kraft paper: Apply a silicon-hydrogen addition type polysiloxane release agent to one side of the kraft paper and cure it after coating. Then apply Wanhua Chemical SA1511 silicone pressure-sensitive adhesive to the other side of the kraft paper and harden it after coating.
[0081] A3. Winding: The kraft paper coated with release agent and pressure-sensitive adhesive is rolled up by a winding roller to form a composite.
[0082] The method for preparing the hydrosilylation type polysiloxane release agent in step A2 specifically comprises the following steps:
[0083] S1. Evenly mix the epoxy-terminated silicone oil, ED-900 polyetheramine and isopropanol, control the temperature at 83°C to react for 3.5 hours, maintain the temperature at 80°C, add 2,3-epoxypropyltrimethylammonium chloride and react for 3 hours to obtain intermediate material A for standby use;
[0084] The mass ratio of the epoxy-terminated silicone oil, ED-900 polyetheramine, isopropyl alcohol and 2,3-epoxypropyltrimethylammonium chloride is 21:2.15:23:0.63;
[0085] S2, vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and Karstedt catalyst are mixed at a mass ratio of 27:49:12:1.6:1.1 at 63°C to obtain intermediate material B for standby use;
[0086] The viscosity of the vinyl-terminated silicone oil is 1000cp;
[0087] The hydrogen-containing silicone oil comprises hydrogen-containing silicone oil with a hydrogen content of 1.6% and hydrogen-containing silicone oil with a hydrogen content of 0.75% in a mass ratio of 2:3;
[0088] The stabilizer comprises SLS, OP-10 and SLS in a mass ratio of 1:2.3:0.5;
[0089] S3. In a nitrogen atmosphere, the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and trifluoromethanesulfonic acid were stirred at 70° C. for 4 h, the temperature was maintained at 75° C., and the intermediate material B was added and reacted for 2 h to obtain a release agent;
[0090] The mass ratio of the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, trifluoromethanesulfonic acid and the intermediate material B is 1:0.3:0.07:1.
[0091] Comparative Example 1
[0092] Compared with Example 3, the difference is that the hydrogen-containing silicone oil in step S2 of Comparative Example 1 is hydrogen-containing silicone oil with a hydrogen content of 1.6%, and the other parameters and operating steps remain unchanged.
[0093] Comparative Example 2
[0094] Compared with Example 3, the difference is that the hydrogen-containing silicone oil in step S2 of Comparative Example 2 is hydrogen-containing silicone oil with a hydrogen content of 0.75%, and the other parameters and operating steps remain unchanged.
[0095] Comparative Example 3
[0096] Compared with Example 3, the difference is that in step S3 of Comparative Example 3, no epoxy-terminated silicone oil and ED-900 polyetheramine are added, and the other parameters and operating steps remain unchanged.
[0097] Comparative Example 4
[0098] Compared with Example 3, the difference is that in step S3 of Comparative Example 4, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane is not added, and the other parameters and operation steps remain unchanged.
[0099] Comparative Example 5
[0100] Compared with Example 3, the difference is that in step S1 of Comparative Example 5, 2,3-epoxypropyltrimethylammonium chloride is not added, and the other parameters and operating steps remain unchanged.
[0101] Comparative Example 6
[0102] Compared with Example 3, the difference is that in step S2 of Comparative Example 6, no SLS is added, the stabilizer includes OP-10 and SLS in a mass ratio of 2.8:1, and the other parameters and operating steps remain unchanged.
[0103] Comparative Example 7
[0104] Compared with Example 3, the difference is that in step S2 of Comparative Example 7, OP-10 is not added, the stabilizer includes SLS and SLS in a mass ratio of 2.2:1.6, and the other parameters and operating steps remain unchanged.
[0105] Comparative Example 8
[0106] Compared with Example 3, the difference is that in step S2 of Comparative Example 8, SLS is not added, the stabilizer includes SLS 45 and OP-10 in a mass ratio of 1.3:2.5, and the other parameters and operating steps remain unchanged.
[0107] Test Example 1
[0108] Peeling force test: The composites prepared by coating and curing the release agent and pressure-sensitive adhesive of Examples 1-3 and Comparative Examples 1-4 were stacked in the order of one composite pressure-sensitive layer close to another composite release layer, with 200 sheets of paper, and the stacked papers were placed in a press, with a set pressure of 20 MPa and a time of 0.75 h. After being taken out, they were cut into 30 mm wide strips in the longitudinal direction; the peeling force test was carried out at a peeling angle of 180° and a peeling speed of 300 mm / min at room temperature. Each sample was measured 5 times, and the results were averaged. The results are shown in Table 1.
[0109] Table 1
[0110] Room temperature peel strength (g / inch) Example 1 29 Example 2 27 Example 3 30 Comparative Example 1 23 Comparative Example 2 21 Comparative Example 3 11 Comparative Example 4 16
[0111] It can be seen from Table 1 that the composite prepared in the present invention has excellent peeling force.
[0112] Test Example 2
[0113] Softness test: Under an environment of 23°C and 65% RH, cut out 35 cm × 35 cm composites obtained by coating and curing the release agent and the pressure-sensitive adhesive of Examples 1-3, Comparative Example 3 and Comparative Example 5, adhere the composites to a PS sheet, peel off the composites with a clamp at a speed of 20 m / min, and observe whether the composites are curled or warped after peeling; the results are shown in Table 2.
[0114] Table 2
[0115]
[0116]
[0117] It can be seen from Table 2 that the composite prepared in the present invention has outstanding softness and resilience, and is easy to rebound and recover when the pressure-sensitive adhesive tape is pulled by external force, and is not easy to deform.
[0118] Test Example 3
[0119] Stability determination:
[0120] (1) Storage stability: The release agents prepared in Examples 1-3 of the present invention and Comparative Examples 6-8 were sealed and stored at room temperature for 3 months to observe whether the release agents had oil bleaching, demulsification, or stratification. The results are shown in Table 3.
[0121] (2) Centrifugal stability: 15 mL of the release agent prepared in Examples 1-3 of the present invention and Comparative Examples 6-8 was poured into a 30 mL test tube and placed in a centrifuge. The tube was centrifuged at 3000 r / min. After 20 min, the emulsion was observed to see if there was oil floating, demulsification, or stratification. The results are shown in Table 3.
[0122] Table 3
[0123]
[0124] It can be seen from Table 3 that the release agent prepared by the present invention has better storage stability and centrifugal stability.
[0125] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0126] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A composite containing a silicone release agent and a pressure-sensitive adhesive, characterized in that: The composite body comprises a release layer, a substrate layer and a pressure-sensitive layer; the release layer is located on one side of the substrate layer, and the pressure-sensitive layer is located on the other side of the substrate layer; The release layer is obtained by coating and curing a release agent, and the release agent is any one of a hydrosilylation-curing polysiloxane release agent, a condensation-curing polysiloxane release agent, a peroxide-curing polysiloxane release agent, and a light-curing polysiloxane release agent; the pressure-sensitive layer is obtained by coating and curing a pressure-sensitive adhesive; the substrate layer is any one of cotton cloth, glass cloth, non-woven fabric, kraft paper, glassine paper, and coated paper; The preparation process of the composite comprises the following steps: A1. Clean, wind and move the substrate layer forward: clean the pollutants on the surface of the substrate layer, wind the cleaned substrate layer on the driving roller of the coating machine, and drive the substrate layer forward with the driving roller; A2. Applying a release agent and a pressure-sensitive adhesive to the substrate layer: applying a release agent to one side of the substrate layer and curing it, and then applying a pressure-sensitive adhesive to the other side of the substrate layer and curing it; A3, winding: the substrate layer coated with the release agent and the pressure-sensitive adhesive is wound up by a winding roller to obtain a composite; The preparation method of the hydrosilylation-curable polysiloxane release agent specifically comprises the following steps: S1. Evenly mix the epoxy-terminated silicone oil, ED-900 polyetheramine and isopropanol, control the temperature for reaction, maintain the temperature, and then add 2,3-epoxypropyltrimethylammonium chloride for reaction to obtain intermediate material A for standby use; The mass ratio of the epoxy-terminated silicone oil, ED-900 polyetheramine, isopropyl alcohol and 2,3-epoxypropyltrimethylammonium chloride is 18-23:1.65-2.15:20-26:0.55-0.72; S2, controlling the temperature and stirring the vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and catalyst to obtain intermediate material B for later use; The stabilizer comprises SLS, OP-10 and SLS in a mass ratio of 1:2-2.5:0.5; S3. In a nitrogen atmosphere, the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and the catalyst are stirred under controlled temperature, and the temperature is maintained. The intermediate material B is added to react to obtain the release agent.
2. The composite body containing an organic silicone release agent and a pressure-sensitive adhesive according to claim 1, characterized in that: The hydrogen-containing silicone oil in step S2 includes hydrogen-containing silicone oil with a hydrogen content of 1.6% and hydrogen-containing silicone oil with a hydrogen content of 0.75%.
3. The composite body containing an organic silicone release agent and a pressure-sensitive adhesive according to claim 2, characterized in that: The mass ratio of the hydrogen-containing silicone oil with a hydrogen content of 1.6% to the hydrogen-containing silicone oil with a hydrogen content of 0.75% is 2:
3.
4. The composite body containing an organic silicone release agent and a pressure-sensitive adhesive according to claim 1, characterized in that: In step S2, the mass ratio of the vinyl-terminated silicone oil, hydrogen-containing silicone oil, stabilizer, N,N-dimethylaminoethyl acrylate and catalyst is 25-30:46-52:10-12:1.2-1.6:1-1.
3.
5. The composite body containing an organic silicone release agent and a pressure-sensitive adhesive as claimed in claim 1, characterized in that: In step S3, the mass ratio of the intermediate material A, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, the catalyst and the intermediate material B is 1:0.3-0.4:0.06-0.07:
1.
6. The composite body containing an organic silicone release agent and a pressure-sensitive adhesive as claimed in claim 5, characterized in that: The catalyst is trifluoromethanesulfonic acid.
Citation Information
Patent Citations
Normal-temperature fast-curing silicone release agent and preparation method thereof
CN108130001A
Preparation method of quaternized polyether segmented modified conductive silver adhesive
CN109517575A
Pressure-sensitive adhesive tape for rubber type lithium battery
CN115353819A
Anchoring agent for fluorosilicone release agent and application of anchoring agent
CN115975428A
Release agent and preparation method thereof
CN117126603A