A nitrogen-containing polymer-supported ruthenium-based catalyst, its preparation and application

By preparing a solid heterogeneous catalyst with a large specific surface area and hierarchical porous structure supporting Ru component in an organic ligand polymer, the problems of difficult catalyst separation in the hydrogen esterification reaction and the high cost and easy deactivation of Pd-based catalysts were solved, achieving high catalytic performance and easy separation, which is suitable for industrial applications.

CN118287147BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410364493.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2026-11-17
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Existing hydrogen esterification reaction systems are homogeneous systems, making it difficult to separate the catalyst from the reactants. Furthermore, existing Pd-based catalytic systems are expensive and prone to agglomeration and deactivation. There is a lack of green, efficient, and recyclable heterogeneous catalysts suitable for industrial applications.

Method used

A solid heterogeneous catalyst is formed by loading a metal Ru component onto an organic ligand polymer, which is generated by self-polymerization of a nitrogen ligand monomer containing vinyl groups or copolymerization with a vinyl sulfonic acid monomer, and then stably binding the component to the polymer backbone through coordination or ionic bonding.

Benefits of technology

It achieves high dispersibility and stability of the catalyst, improves catalytic reaction performance, and makes the catalyst easy to separate from reactants and products, thus having broad prospects for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118287147B_ABST
    Figure CN118287147B_ABST
Patent Text Reader

Abstract

This invention relates to a solid heterogeneous catalyst, its preparation method, and its applications. The catalyst comprises a metal component and an organic ligand polymer. The metal component is Ru, and the organic ligand polymer is a polymer with a large specific surface area and hierarchical porous structure, formed by the self-polymerization of a vinyl-containing nitrogen ligand monomer or by solvothermal copolymerization with a vinyl sulfonic acid monomer. The metal component forms coordinate or ionic bonds with the nitrogen atoms in the organic ligand polymer backbone, and exists in a highly dispersed and stable manner on the organic ligand polymer support. In hydrogen esterification reactions, the catalyst of this invention is easily separated from the reactants and products, and has broad industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a solid heterogeneous catalyst for hydrogen esterification reactions, its preparation method and application, belonging to the field of heterogeneous catalysis technology. Background Technology

[0002] Homogeneous catalytic systems exhibit high catalytic activity and selectivity for the target product under milder reaction conditions, but separation of the catalyst from the reactants is difficult.

[0003] The biggest advantage of heterogeneous catalysis compared to homogeneous catalysis is the ease of separation between the catalyst and reactants. However, its main drawbacks include demanding reaction conditions and relatively low reactivity. Therefore, developing novel supported heterogeneous catalysts that combine the advantages of both homogeneous and heterogeneous catalysis is a hot topic in scientific research.

[0004] In recent years, the design and synthesis of porous organic polymer materials has gradually become one of the new hot topics in the field of porous materials research. Compared with traditional inorganic microporous materials and metal-organic frameworks (MOFs), the framework of organic microporous polymers is composed of pure organic molecules connected by covalent bonds, and has open channels and excellent pore properties.

[0005] More importantly, the diversity of organic chemical synthesis methods provides a wealth of synthetic routes and construction methods for building organic molecular networks. By purposefully introducing functionalized organic molecules, materials can acquire corresponding properties, and by adjusting the structure of organic molecules, the pore properties of materials can be controlled.

[0006] In addition, metal-functionalized porous organic polymer materials can introduce catalytically active metal units into porous organic polymers, achieving high dispersion in the organic copolymer carrier in the form of single atoms. This not only helps to stabilize the metal active sites, but also greatly improves the utilization efficiency of the metal.

[0007] The reaction of alcohols, alkenes, and CO to prepare esters via catalyst is called hydrogen esterification. The resulting esters have a wide range of applications in the industrial field. They can be used as intermediates in organic synthesis and in the manufacture of fragrances. Esters are also excellent solvents, used in the manufacture of cellulose ethers and esters, and as solvents for various natural and synthetic resins.

[0008] However, existing hydrogen esterification reaction systems are all homogeneous, making it difficult to separate the catalyst from the reaction liquid. Furthermore, existing catalysts for olefin hydrogen esterification reactions are mainly Pd-based systems. In comparison, Ru-based systems are a promising application direction. Unlike Pd, which is expensive and prone to agglomeration and deactivation, Ru is a good alternative metal.

[0009] In summary, for hydrogen esterification reactions applicable to practical industrial applications, green, efficient, and recyclable heterogeneous catalysts are the main research direction in this field. Summary of the Invention

[0010] To address the aforementioned problems, the present invention aims to provide a solid heterogeneous catalyst consisting of an organic ligand polymer supporting a metal active component, its preparation method, and its application.

[0011] Therefore, the present invention provides a solid heterogeneous catalyst for hydrogen esterification reaction, characterized in that: the organic ligand polymer is a polymer with a large specific surface area and a hierarchical porous structure generated by self-polymerization of a vinyl nitrogen ligand monomer or by solvothermal copolymerization with a vinyl sulfonic acid monomer.

[0012] The metal component is Ru, and the organic ligand polymer is a polymer with a large specific surface area and a hierarchical porous structure, which is generated by the self-polymerization of a vinyl nitrogen ligand monomer or by solvothermal copolymerization with a vinyl sulfonic acid monomer. The metal component forms coordination bonds or ionic bonds with the N atoms in the organic ligand polymer backbone and exists in a highly dispersed and stable manner on the organic ligand polymer carrier.

[0013] In a preferred embodiment, the metal component accounts for 0.05-20.0% of the total weight of the solid heterogeneous catalyst.

[0014] In a preferred embodiment, the vinyl-containing nitrogen ligand is selected from one or more of the following: .

[0015] In a preferred embodiment, the organic ligand polymer has a specific surface area of ​​300-2800 m². 2 / g, pore volume 0.2-5.0 cm³ 3 / g, with a pore size distribution of 0.3-80.0 nm.

[0016] In a preferred embodiment, the preparation method of the solid heterogeneous catalyst includes the following steps: a) adding a free radical initiator to a solvent containing a vinyl nitrogen ligand monomer at 273-473 K and an inert gas protective atmosphere, and then adding or not adding a vinyl sulfonic acid monomer, and stirring for 0.5-100 hours; b) allowing the solution from step a) to stand in a hydrothermal autoclave for 0.5-100 hours at 273-473 K and an inert gas protective atmosphere to carry out a solvothermal polymerization reaction; c) after step b) is completed, removing the solvent under vacuum at a temperature of 273-473 K to obtain the organic ligand polymer; d) placing the organic ligand polymer in a solvent containing an active metal component, stirring for 0.5-100 hours at 273-473 K and an inert gas protective atmosphere, and then removing the solvent under vacuum at a temperature of 273-473 K to obtain the solid heterogeneous catalyst with the active metal component supported by the organic ligand polymer.

[0017] In a preferred embodiment, the solvent used in steps a) and d) of the catalyst preparation method is one or more of benzene, toluene, tetrahydrofuran, methanol, ethanol, dichloromethane, dichloroethane, or deionized water; the free radical initiator used in step a) is one or more of cyclohexanone peroxide, benzoyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, or azobisisoheptanenitrile.

[0018] In a preferred embodiment, the weight ratio of the free radical initiator to the organic monomer in the catalyst preparation method is 1:500-1:5.

[0019] In a preferred embodiment, the application of the solid heterogeneous catalyst in the hydrogen esterification reaction refers to carrying out the hydrogen esterification reaction of an alcohol feedstock and an olefin / CO mixture in a fixed bed, trickle bed, slurry bed, or batch reactor in the presence of the solid heterogeneous catalyst, wherein the reaction temperature is 273-573 K, the reaction pressure is 0.05-20.0 MPa, and the liquid hourly space velocity is 0.01-20.0 h⁻¹. -1 The gas space velocity is 100-20000 h⁻¹ -1 .

[0020] In a preferred embodiment, the inert gas atmosphere during the synthesis of the organic ligand polymer is one or more of argon, helium, and nitrogen.

[0021] The beneficial effects of this invention include, but are not limited to, the following: Compared with existing hydrogen esterification catalysts, the solid heterogeneous catalyst of this invention has a simpler preparation method; the metal component and the N atoms in the polymer support exist stably on the support due to coordination; the polymer support has a large specific surface area and a hierarchical porous structure, allowing the metal component to exist in a highly dispersed manner on the support, thus giving the solid heterogeneous catalyst of this invention excellent catalytic performance and high stability. Furthermore, the catalyst of this invention is a heterogeneous catalyst on a macroscopic scale, therefore it has significant advantages in recycling and separation from reactants and products, and has broad prospects for industrial application. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the synthesis route of the solid heterogeneous catalyst of the present invention.

[0023] Figure 2 This is a schematic diagram of another solid heterogeneous catalyst synthesis route of the present invention.

[0024] Figure 3 The figures show the N2 adsorption-desorption isotherm and pore size distribution curve of the catalyst of this invention. Detailed Implementation

[0025] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0026] Unless otherwise specified, all raw materials and reagents used in this application are commercially purchased and used directly without processing. The instruments and equipment used adopt the manufacturer's recommended scheme and parameters.

[0027] In the examples, all catalyst evaluation results were analyzed using an Agilent 7890B liquid chromatograph with an FID detector, capillary column, and internal standard method to determine the liquid phase composition, with 1,4-dioxane or toluene as the internal standard.

[0028] Product selectivity is calculated based on the composition of each product.

[0029] In the embodiments of this application, the conversion rate of olefins and the selectivity of products are calculated based on the number of carbon moles of the converted olefins.

[0030] Example 1 Under an argon atmosphere at 298 K, 5.0 g of tris(4-vinylbenzene)nitrogen (i.e., the L1 ligand) was dissolved in 60 mL of tetrahydrofuran solvent. 0.25 g of azobisisobutyronitrile (AIBN) free radical initiator was added to the solution, and the mixture was stirred for 0.5 h. The stirred solution was then transferred to a hydrothermal autoclave and polymerized at 373 K under an inert gas atmosphere using a solvothermal method for 24 h. After polymerization, the mixture was cooled to room temperature, and the solvent was removed under vacuum at 333 K to obtain the corresponding porous organic polymer. The specific surface area of ​​this organic ligand polymer was 2030 m². 2 / g, pore volume 2.6cm 3 / g, with a pore size distribution of 0.7-35.0 nm.

[0031] Under an inert gas atmosphere at 298 K, 0.0156 g of p-cymene ruthenium(II) dichloride dimer was dissolved in 40 mL of tetrahydrofuran solvent, and 1.0 g of the porous organic polymer prepared above was added. The mixture was stirred for 24 hours. Subsequently, the solvent was removed under vacuum at 333 K to obtain a solid heterogeneous catalyst with a metal component supported on an organic ligand polymer. Ru accounts for 1.0% of the total weight of this solid heterogeneous catalyst. A schematic diagram of the synthesis route for the solid heterogeneous catalyst of this invention is shown below. Figure 1 The N2 adsorption-desorption isotherms and pore size distribution curves of the solid heterogeneous catalyst of the present invention are shown in the figure. Figure 3 The results showed that this catalyst possesses a good specific surface area and a rich hierarchical porous structure. Specific reaction results are shown in Table 1.

[0032] Example 2 In Example 2, except that 0.0312 g of p-cymene ruthenium(II) chloride dimer was used to replace 0.0156 g of p-cymene ruthenium(II) chloride dimer, the rest of the catalyst preparation process and conditions were the same as in Example 1. Specific reaction results are shown in Table 1.

[0033] Example 3 In Example 3, except that 0.0176 g of ruthenium chloride trihydrate (III) was used to replace 0.0156 g of p-cymene ruthenium chloride (II) dimer, the catalyst preparation process and conditions were the same as in Example 1. Specific reaction results are shown in Table 1.

[0034] Example 4 In Example 4, except that 0.0145 g of ruthenium acetate (III) was used to replace 0.0156 g of p-cymene ruthenium dichloride (II) dimer, the catalyst preparation process and conditions were the same as in Example 1. Specific reaction results are shown in Table 1.

[0035] Example 5 In Example 5, the polymer synthesis process was identical to that in Example 1, except that dichloromethane was used in place of tetrahydrofuran solvent by an equal volume. Specific reaction results are shown in Table 1.

[0036] Example 6 In Example 6, the polymer synthesis process was the same as in Example 1, except that 12 hours of stirring was replaced with 0.5 hours of stirring. Specific reaction results are shown in Table 1.

[0037] Example 7 In Example 7, the catalyst preparation process and conditions were the same as in Example 1, except that benzoyl peroxide was used instead of azobisisobutyronitrile as the free radical initiator. Specific reaction results are shown in Table 1.

[0038] Example 8 In Example 8, except that the crosslinking agent polypropylene glycol was used instead of the free radical initiator azobisisobutyronitrile, the rest of the catalyst preparation process and conditions were the same as in Example 1. Specific reaction results are shown in Table 1.

[0039] Example 9 In Example 9, the catalyst preparation process and conditions were the same as in Example 1, except that 5.0 g of tris(4-vinylphenyl)nitrogen (i.e., L1 ligand) was replaced with 5.0 g of tris(3-vinylphenyl)nitrogen (i.e., L2 ligand). Specific reaction results are shown in Table 1.

[0040] Example 10 In Example 10, the catalyst preparation process and conditions were the same as in Example 1, except that 5.0 g of tris(4-vinylphenyl)nitrogen (i.e., L1 ligand) was replaced with 4.0 g of tetra(4-vinylphenyl)nitrogen bromide (i.e., L7 ligand) and 1.0 g of a mixture of vinylsulfonic acid monomers. Specific reaction results are shown in Table 1, and a schematic diagram of the synthesis route of the solid heterogeneous catalyst of this invention is shown below. Figure 2 .

[0041] Example 11 In Example 11, the catalyst preparation process and conditions were the same as in Example 1, except that 5.0 g of tris(4-vinylphenyl)nitrogen (i.e., L1 ligand) was replaced with 4.0 g of tris(4-vinylphenyl)nitrogen iodide (i.e., L6 ligand) and 1.0 g of a mixture of vinylsulfonic acid monomers. Specific reaction results are shown in Table 1.

[0042] Example 12 0.05 g of the solid heterogeneous catalyst prepared in Example 1 was loaded into a high-pressure autoclave reactor. 2 mmol of 1-pentene and 5 g of methanol were added sequentially. The reactor was sealed, and CO was introduced to 3 MPa (olefin / CO molar ratio of 1 / 20). The temperature was slowly increased to 100 °C under temperature control, and the reaction was carried out for 24 h. After the reaction, the reactor was cooled to room temperature, and excess reaction gas was slowly released. The catalyst was separated by filtration. The obtained product was added toluene as an internal standard and analyzed by an HP-7890N gas chromatograph equipped with an HP-5 capillary column and an FID detector. The conversion rate of 1-pentene was 81%, the yield of methyl hexanoate was 76%, and the TON was 1200. Specific reaction results are shown in Table 1.

[0043] Comparative Example 1 Under an argon atmosphere at 298 K, 5.0 g of tris(4-vinylbenzene)benzene (without coordinating nitrogen atoms) was dissolved in 60 mL of tetrahydrofuran solvent. 0.25 g of azobisisobutyronitrile (AIBN) free radical initiator was added to the solution, and the mixture was stirred for 0.5 hours. The stirred solution was transferred to a hydrothermal autoclave and polymerized at 373 K under an inert gas atmosphere using a solvothermal method for 24 hours. After polymerization, the solution was cooled to room temperature, and the solvent was removed under vacuum at 333 K to obtain the corresponding porous organic polymer. Under an inert gas atmosphere at 298 K, 0.0156 g of p-cymene ruthenium(II) dichloride dimer was dissolved in 40 mL of tetrahydrofuran solvent. 1.0 g of the porous organic polymer prepared above was added, and the mixture was stirred for 24 hours. Subsequently, the solvent was removed under vacuum at 333 K to obtain the corresponding organic polymer-supported metal component solid heterogeneous catalyst. Ru constitutes 1.0% of the total weight of this solid heterogeneous catalyst. Comparative experimental results show that the core of the catalyst in this invention lies in the synergistic participation of the ruthenium-nitrogen coordination system in the reaction, and ordinary polymer-supported ruthenium cannot achieve the reaction effect of this patent.

[0044] The catalysts obtained in Examples 1-12 and the comparative examples were evaluated in a continuous reactor such as a 30 mL batch reactor or a fixed bed reactor.

[0045] In this process, a catalyst is added to the reactor, followed by the simultaneous addition of methanol, olefins, and CO, and the reaction temperature is raised to allow for further reaction. Alternatively, a catalyst is added to the reaction tube of a continuous reactor, such as a fixed-bed, fluidized-bed, or trickle-bed reactor, and methanol, olefins, and CO are continuously introduced and the reaction temperature is raised to allow for further reaction. After the reaction, samples are taken for analysis, and the conversion rate of olefins is calculated. The results are detailed in Table 1.

[0046] Table 1. Results of olefin hydrogen esterification reaction Example Olefins alcohols Ester yield % Ester TON 1 ethylene methanol 79% 1300 2 ethylene methanol 78% 1280 3 ethylene methanol 77% 1260 4 ethylene methanol 83% 1360 5 propylene methanol 75% 1070 6 1-Butene methanol 80% 1140 7 propylene methanol 78% 1120 8 ethylene methanol 79% 1300 9 ethylene methanol 77% 1105 10 1-Butene methanol 81% 1150 11 propylene ethanol 77% 1100 12 methanol 76% 1200 Comparative Example 1 ethylene methanol 23% 378 Note: The hydrogen esterification product of each type of olefin is an ester compound with one more carbon atom. For example, the product of ethylene and methanol with carbon monoxide is methyl propionate, the product of propylene and methanol with carbon monoxide is methyl butyrate, and so on.

[0047] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses the above-described preferred embodiments, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

[0048] The metal component forms coordination or ionic bonds with the nitrogen atoms in the organic ligand polymer backbone, existing in a highly dispersed and stable manner on the organic ligand polymer support. In the hydrogen esterification reaction, the catalyst of this invention, on the one hand, is stably present on the support due to coordination or ionic bonds between the metal component and the nitrogen atoms in the polymer support; on the other hand, the polymer support has a large specific surface area and a hierarchical porous structure, allowing the metal component to exist in a highly dispersed manner on the support. Therefore, the solid heterogeneous catalyst of this invention exhibits excellent catalytic performance and stability, and the catalyst is easily separated from reactants and products, showing broad prospects for industrial application.

Claims

1. The application of a solid heterogeneous catalyst in the reaction of olefins and alcohols to produce esters, the catalyst comprising a metal component and an organic ligand polymer, wherein the metal component is metal Ru, and the organic ligand polymer is a polymer generated by self-polymerization of a vinyl-containing nitrogen ligand monomer or by solvothermal copolymerization of a vinyl-containing nitrogen ligand monomer and a vinyl sulfonic acid monomer; wherein the metal component forms coordinate or ionic bonds with the N atoms in the backbone of the organic ligand polymer and exists on the organic ligand polymer support. The vinyl-containing nitrogen ligand is selected from one or more of the following: , The olefin is one of ethylene, propylene, 1-butene, and 1-pentene.

2. The application according to claim 1, characterized in that: The Ru accounts for 0.05-20.0% of the total weight of the solid heterogeneous catalyst.

3. The application according to claim 1, characterized in that: The Ru accounts for 0.1-10.0% of the total weight of the solid heterogeneous catalyst.

4. The application according to claim 1, characterized in that: The Ru accounts for 0.2-6.0% of the total weight of the solid heterogeneous catalyst.

5. The application according to claim 1, characterized in that: The specific surface area of ​​the organic ligand polymer is 300-2800 m². 2 / g, pore volume 0.2-5.0 cm³ 3 / g, with a pore size distribution of 0.3-80.0 nm.

6. The application according to any one of claims 1-5, characterized in that, include: a) At 223~473 K, under an inert atmosphere, in an organic solvent, add a nitrogen ligand monomer containing vinyl groups, with or without vinyl sulfonic acid monomers, with or without crosslinking agents, and then add a free radical initiator. After mixing, stir the mixture for 0.3~5 hours. The inert gas in the inert atmosphere is one or more of argon, helium, and nitrogen. b) Transfer the mixed solution obtained in step a) to a high-pressure reactor for synthesis. Under an inert gas atmosphere at 273K~473K, carry out the polymerization reaction by solvothermal polymerization and let it stand for 1~80 hours to obtain a nitrogen-containing porous organic polymer. c) The polymer obtained in step b) is subjected to vacuum removal of solvent at room temperature to obtain an organic polymer containing exposed nitrogen with a hierarchical porous structure, which is the support for the heterogeneous catalyst. In step a), when vinyl sulfonic acid is added, the molar ratio of the vinyl-containing nitrogen ligand monomer to the vinyl sulfonic acid monomer is 0.01:1 to 10:

1. In step a), the molar ratio of the vinyl-containing nitrogen ligand monomer to the crosslinking agent is 0.01:1 to 10:1 when a crosslinking agent is added. Before polymerization into organic polymers, the concentration of the vinyl nitrogen ligand monomer in the organic solvent ranges from 0.01 to 1000 g / L.

7. The application according to claim 6, characterized in that, Step a) At 273~423 K, under an inert atmosphere, add a vinyl nitrogen ligand monomer, with or without vinyl sulfonic acid monomer, with or without crosslinking agent, and then add a free radical initiator to an organic solvent. After mixing, stir the mixture for 0.3~5 hours. The inert gas in the inert atmosphere is one or more of argon, helium, and nitrogen. Step b) Transfer the mixed solution obtained in step a) to a high-pressure reactor for synthesis. Under an inert gas atmosphere at 273~423 K, perform a solvothermal polymerization reaction and let it stand for 1~80 hours to obtain a nitrogen-containing porous organic polymer. In step a), when vinyl sulfonic acid is added, the molar ratio of the vinyl-containing nitrogen ligand monomer to the vinyl sulfonic acid monomer is 0.05:1 to 8:

1. In step a), the molar ratio of the vinyl-containing nitrogen ligand monomer to the crosslinking agent is 0.1:1 to 10:1 when a crosslinking agent is added. Before polymerization into organic polymers, the concentration of the vinyl nitrogen ligand monomer in the organic solvent ranges from 0.05 to 500 g / L.

8. The application according to claim 6, characterized in that, Step a) At 313~403 K, under an inert atmosphere, add a vinyl nitrogen ligand monomer, with or without vinyl sulfonic acid monomer, with or without crosslinking agent, and then add a free radical initiator to an organic solvent. After mixing, stir the mixture for 0.3~5 hours. The inert gas in the inert atmosphere is one or more of argon, helium, and nitrogen. Step b) Transfer the mixed solution obtained in step a) to a high-pressure reactor for synthesis. Under an inert gas atmosphere at 313~403 K, perform a solvothermal polymerization reaction and let it stand for 1~80 hours to obtain a nitrogen-containing porous organic polymer. In step a), the molar ratio of the vinyl-containing nitrogen ligand monomer to the vinyl sulfonic acid monomer is 0.1:1 to 6:1 when vinyl sulfonic acid is added. In step a), the molar ratio of the vinyl-containing nitrogen ligand monomer to the crosslinking agent is 0.2:1 to 10:1 when a crosslinking agent is added. Before polymerization into organic polymers, the concentration of the vinyl nitrogen ligand monomer in the organic solvent ranges from 0.1 to 200 g / L.

9. The application according to claim 6, characterized in that, The solvents used in steps a) and b) are one or more of benzene, toluene, tetrahydrofuran, methanol, ethanol, dichloromethane, dichloroethane, or deionized water; The free radical initiator used in step a) is one or more of cyclohexanone peroxide, benzoyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, or azobisisoheptanenitrile; The molar ratio of the vinyl nitrogen ligand monomer to the free radical initiator is 300:1 to 10:

1.

10. The application according to claim 9, characterized in that, In step a), the molar ratio of the vinyl nitrogen ligand monomer to the free radical initiator is 200:1 to 20:

1.

11. The application according to claim 9, characterized in that, In step a), the molar ratio of the vinyl nitrogen ligand monomer to the free radical initiator is 100:1 to 30:

1.

12. The application according to claim 6, characterized in that, The crosslinking agent is one or more of the following: polyethylene glycol, polypropylene glycol, trimethylolpropane, trimethylolethane, trimethoxysilane, dicumyl peroxide, bis(2,4-dichlorobenzoyl peroxide), and hydroxypropyl acrylate.

13. The application according to claim 1, characterized in that, In the presence of the aforementioned solid heterogeneous catalyst, an alcohol feedstock is subjected to a hydrogen esterification reaction with an olefin / CO mixture in a fixed-bed, trickle-bed, slurry-bed, or batch reactor. The reaction temperature in these reactor types is 273-573 K, the reaction pressure is 0.05-20.0 MPa, and the liquid hourly space velocity is 0.01-20.0 h⁻¹. -1 The gas space velocity is 100-20000 h⁻¹ -1 The molar ratio of the olefin feedstock to the CO feedstock is 1:1 to 1:

100.

14. The application according to claim 13, characterized in that, In several types of reaction apparatus, the reaction temperature is 303K-503K, the reaction pressure is 0.2-10.0MPa, and the liquid hourly space velocity is 0.03-15 h⁻¹. -1 The gas space velocity is 300-15000 h. -1 The molar ratio of the olefin feedstock to the CO feedstock is 1:1 to 1:

50.

15. The application according to claim 13, characterized in that, In several types of reaction apparatus, the reaction temperature is 353K-473K, the reaction pressure is 0.5-6MPa, and the liquid hourly space velocity is 0.05-10 h⁻¹. -1 The gas space velocity is 500-10000 h⁻¹ -1 The molar ratio of the olefin feedstock to the CO feedstock is 1:1 to 1:

20.

16. The application according to claim 1 or 13, characterized in that, The alcohols are selected from one or more of the following alcohols: methanol, ethanol, n-propanol, isopropanol, butanol, isobutanol, pentanol, isopentanol, hexanol, isohexanol, heptanol, isohexanol, octanol, isooctanol, nonanol, isononol, decol, and isodecanol.

Citation Information

Patent Citations

  • Organic nitrogen-containing polymer carrier Rh-loading catalyst as well as preparation and application thereof

    CN109453812A

  • Method for synthesizing methyl isononanoate from diisobutylene