A method for preparing silver-based active solder foil

The low melting point mixture of silver-based alloy powder and titanium powder is prepared by vacuum smelting and atomization, combined with low-temperature sintering and hot-rolling processes, which solves the problem of silver-based solder reacting at high temperatures to generate brittle intermetallic compounds, and realizes solder foil. The densification and extremely thin thickness preparation avoid brittle fracture and cracking defects.

CN118287678BActive Publication Date: 2024-10-18CHONGQING MATERIALS RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410408091.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-18
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

During the high-temperature process of existing silver-based solders, titanium reacts with silver and other elements to form brittle intermetallic compounds, resulting in poor formability of the solder foil, making it difficult to process to extremely thin thickness (≤0.02mm) and prone to brittle fracture and cracking defects.

Method used

Vacuum melting and atomization are used to prepare a low melting point mixture of silver-based alloy powder and titanium powder. The sintering and hot-rolling process is below 600°C to avoid the generation of brittle intermetallic compounds. The foil is ensured through multiple passes of cold rolling and annealing. Denseness and thinness.

Benefits of technology

The densification of the solder foil was achieved, brittle fracture and cracking defects were avoided, and a silver-based active solder foil with a thickness of ≤0.02mm was successfully prepared, ensuring its stability after multiple deformation processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118287678B_ABST
    Figure CN118287678B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a silver-based active solder foil. The method adopts vacuum melting and atomization to prepare alloy powder. After measuring the melting point temperature of the alloy powder, the alloy powder is mixed with titanium powder, molded, sintered, hot-rolled, surface treated, cold-rolled to the thickness of the finished product, and then annealed. According to the method of the invention, silver and one or more elements of copper, gold, tin, lead, and indium are vacuum melted and atomized to prepare alloy powder, and then mixed with titanium powder, sintered and hot-rolled at a temperature lower than that of a traditional process (600°C), effectively avoiding the generation of brittle intermetallic compounds, realizing the densification of the alloy blank, and no defects such as brittle fracture and cracking will occur after multiple deformation processes, and the thickness of the prepared solder foil is less than or equal to 0.02 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foil processing and preparation, and in particular relates to a method for preparing a silver-based active solder foil. Background Art

[0002] In the fields of aerospace, energy and chemical engineering, metallurgy and machinery, metal materials and ceramic materials are connected to form composite components to give full play to the advantages of both materials.

[0003] At present, the connection between metal materials and ceramic materials uses silver-based titanium-containing solder to weld metal and ceramic or graphite (diamond). The titanium element in the solder can react with the oxygen element or carbon element in the ceramic or graphite (diamond) to improve the wettability and fluidity of the solder at the welding interface. It is a key active material for welding metal and ceramic or graphite (diamond). However, the active element titanium is added to the silver-based solder, and the following two preparation processes are generally used: 1. Mixing, molding, sintering, and processing; 2. Melting, casting, and processing. In the above two processes, the melting point of the alloy is relatively high. In the high-temperature process (such as melting, sintering, etc.), when the temperature exceeds 600°C, the titanium element reacts with silver and other elements to form brittle intermetallic compounds, resulting in poor forming performance of the alloy. After multiple deformation processes, defects such as brittle fracture and cracking occur, and the thickness of the solder foil cannot be processed to ≤0.02mm. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a silver-based active solder foil in view of the deficiencies in the prior art, which realizes the densification of the alloy billet during sintering and hot rolling at a temperature below 600°C, avoids the formation of brittle intermetallic compounds, and does not cause defects such as brittle fracture and cracking after multiple deformation processes. The thickness of the solder foil is ≤0.02mm.

[0005] The object of the present invention is achieved in that:

[0006] A method for preparing a silver-based active solder foil comprises the following steps:

[0007] 1) Preparation of pre-alloyed powder:

[0008] Silver and one or more elements of copper, gold, tin, lead and indium are vacuum melted and atomized to prepare spherical or quasi-spherical alloy powders;

[0009] 2) Melting point test:

[0010] Test steps 1) obtaining the melting point temperature of the alloy powder;

[0011] 3) Mixing:

[0012] In an argon or helium atmosphere, the alloy powder of step 1) is mixed with titanium powder, wherein the amount of titanium powder added is 1% to 5% of the total weight, and metal balls are added during the mixing;

[0013] 4) Molding:

[0014] The mixed powder is pressed into shape at a pressure of 80-120Mpa for 30-90s.

[0015] 5) Sintering:

[0016] Sintering under vacuum or protective atmosphere, sintering temperature = melting point temperature × 0.6-0.7, sintering time is 30-60min, the sintering temperature is calculated according to the melting point temperature in step 2);

[0017] 6) Hot rolling

[0018] Hot rolling to a thickness of 0.2-0.5 mm, hot rolling blanking temperature = sintering temperature × 0.8-0.9, the hot rolling blanking temperature is calculated according to the sintering temperature in step 5);

[0019] 7) Surface treatment:

[0020] The blank after hot rolling is polished and ground to remove impurities such as surface oxide scale;

[0021] 8) Cold rolling and annealing:

[0022] The surface treated blank is subjected to multiple cold rolling passes, and annealing treatment is performed after every 4-6 passes. After cold rolling to the target size, annealing treatment is performed again.

[0023] Step 1) The vacuum melting temperature is 900-1200°C and the vacuum degree is 1×10 -1 Pa, the vacuum degree of atomization is 1-10Pa, and the gas pressure of atomization is 3-7Mpa.

[0024] Step 3) The alloy powder and titanium powder are placed in a silver alloy or copper alloy tank for mixing.

[0025] The alloy powder has a particle size of 5-30 μm, the titanium powder is spherical or quasi-spherical, has a purity of 99.9%, and a particle size of 5-30 μm.

[0026] Step 3) The metal balls are made of silver or copper, and the amount of the metal balls added is 20%-40% of the total weight of the alloy powder.

[0027] Step 3) The mixing speed is 10-60r / min and the mixing time is 6-12h.

[0028] Step 6) The deformation amount of each hot rolling pass is 30-40%.

[0029] Step 8) The deformation amount of each cold rolling pass is 10%-20%.

[0030] Step 8) The annealing treatment is performed at a temperature of 300-400°C and for 30 minutes.

[0031] Beneficial effects of the present invention:

[0032] (1) The alloy powder prepared by vacuum melting and atomization in the present invention has a low melting point;

[0033] (2) The present invention adopts the above alloy powder and titanium powder to mix and then form, sinter and hot roll. Since the melting point of the alloy powder is relatively low, the temperature of sintering and hot rolling is lower than the temperature of the traditional process (600°C), which effectively avoids the reaction of titanium element with silver and other elements to produce brittle metal compounds, realizes the densification of the alloy powder and titanium powder alloy billet, and will not have defects such as brittle fracture and cracking after multiple deformation processes;

[0034] (3) The present invention can produce solder foil with a thickness of ≤0.02 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a flow chart of the present invention;

[0036] Figure 2 The foil material of the present invention has a thickness of 0.02 mm;

[0037] Figure 3 This is the cross section of the foil with a thickness of 0.02 mm according to the present invention. DETAILED DESCRIPTION

[0038] Further description is given below in conjunction with the accompanying drawings and specific implementation methods.

[0039] Embodiment 1:

[0040] Preparation of AgCu with a thickness of 0.018 mm 30 Sn1Ti 1.5 Alloy foil, see Figure 1 , including the following steps:

[0041] 1) Preparation of pre-alloyed powder:

[0042] Prepare silver-copper-tin alloy powder, with a total weight of 1 kg, and prepare according to the weight ratio, silver 67.5wt%, copper 30wt%, tin 1wt%, and the purity of the silver, copper, and tin is 99.99%. Place the ingredients in a vacuum melting furnace for melting and atomization, the melting temperature is 1000℃, and the melting vacuum is 1×10 -1 Pa, the vacuum degree during atomization is better than 2Pa, the atomization gas pressure is 4Mpa, and the silver-copper-tin alloy spherical powder is collected after atomization and cooling;

[0043] 2) Melting point test:

[0044] The melting point of the silver-copper-tin alloy powder obtained in step 1) is 775° C. as measured by thermal analysis.

[0045] 3) Mixing:

[0046] The silver-copper-tin alloy spherical powder collected in step 1) and the spherical or quasi-spherical titanium powder are placed in a copper alloy tank, and mixed under an argon protective atmosphere, wherein the amount of titanium powder added is 1.5wt%, and copper balls are added during mixing, wherein the amount of balls added is 25% of the total weight of the alloy powder, about 250g; the purity of the titanium powder is 99.9%, the particle size range is 5-20μm, the mixing speed is 40r / min, and the mixing time is 8h;

[0047] 4) Molding:

[0048] The mixed powder is loaded into a rectangular rubber mold and statically pressed with a molding pressure of 100 MPa and a holding time of 60 seconds.

[0049] 5) Sintering:

[0050] The formed alloy was sintered in vacuum, the sintering temperature = 775 × 0.6 = 465 ° C, and the sintering time was 60 min;

[0051] 6) Hot rolling:

[0052] The sintered alloy is gradually hot rolled to a thickness of 0.2 mm, the hot rolling blanking temperature = 465 × 0.9 = 418.5 ° C, and the deformation of each hot rolling pass is 30%;

[0053] 7) Surface treatment:

[0054] The hot-rolled blank is polished and ground to remove impurities such as oxide scale on its surface;

[0055] 8) Cold rolling and annealing:

[0056] The blank after surface treatment is cold rolled, and the deformation of each cold rolling pass is 10%-20%. After every 4 cold rolling passes, it needs to be annealed in vacuum or protective atmosphere, and then annealed again after rolling to the target size;

[0057] Processing thickness: 0.2mm→0.16mm→0.128mm→0.1mm→400℃×30min annealing→0.082mm→0.066mm→0.052mm→0.042mm→350℃×30min annealing→0.034mm→0.027mm→0.025mm→0.022mm→350℃×30min annealing→0.018mm→300℃×30min annealing.

[0058] Embodiment 2:

[0059] Preparation of AgCu with a thickness of 0.02 mm 30 Sn 0.5 Au 0.5 Ti2 alloy foil, see Figure 1 , including the following steps:

[0060] 1) Preparation of pre-alloyed powder:

[0061] Prepare silver-copper-tin-gold alloy powder, with a total weight of 1 kg, and prepare according to the weight ratio, silver 67wt%, copper 30wt%, tin 0.5wt%, gold 0.5wt%, and the purity of the silver, copper, tin, and gold is 99.99%. Place the ingredients in a vacuum melting furnace for melting and atomization, the melting temperature is 1000℃, and the melting vacuum is 1×10 -1 Pa, the vacuum degree during atomization is better than 2Pa, the atomization gas pressure is 4Mpa, and the silver-copper-tin-gold alloy spherical powder is collected after atomization cooling;

[0062] 2) Melting point test:

[0063] The melting point of the silver-copper-tin-gold alloy spherical powder obtained in step 1) is 778° C. by thermal analysis.

[0064] 3) Mixing:

[0065] The silver-copper-tin-gold alloy spherical powder collected in step 1) and the spherical or quasi-spherical titanium powder are placed in a copper alloy tank, and mixed under an argon protective atmosphere, wherein the amount of titanium powder added is 2wt%, and copper balls are added during mixing, wherein the amount of balls added is 25% of the weight of the alloy powder, about 250g; the purity of the titanium powder is 99.9%, the particle size range is 5-20μm, the mixing speed is 40r / min, and the mixing time is 8h;

[0066] 4) Molding:

[0067] The mixed powder is loaded into a rectangular rubber mold and statically pressed with a molding pressure of 100 MPa and a holding time of 60 seconds.

[0068] 5) Sintering:

[0069] The formed alloy was sintered in vacuum, the sintering temperature = 778 × 0.6 = 467 ° C, and the sintering time was 60 min;

[0070] 6) Hot rolling:

[0071] The sintered alloy is gradually hot rolled to a thickness of 0.2 mm, the hot rolling blanking temperature = 467 × 0.9 = 420 ° C, and the deformation of each hot rolling pass is 30%;

[0072] 7) Surface treatment:

[0073] The hot-rolled blank is polished and ground to remove impurities such as oxide scale on its surface;

[0074] 8) Cold rolling and annealing:

[0075] The blank after surface treatment is cold rolled, and the deformation of each cold rolling pass is 10%-20%. After every 4 cold rolling passes, it needs to be annealed in vacuum or protective atmosphere, and then annealed again after rolling to the target size;

[0076] Processing thickness: 0.2mm→0.16mm→0.128mm→0.1mm→400℃×30min annealing→0.082mm→0.066mm→0.052mm→0.042mm→350℃×30min annealing→0.034mm→0.027mm→0.025mm→0.02mm→300℃×30min annealing.

[0077] The melting point temperature, sintering temperature and hot rolling temperature of the alloy powders of Example 1 and Example 2 are as follows:

[0078] Alloy powder melting point temperature Sintering temperature Hot rolling temperature Foil thickness Example 1 778℃ 467℃ 420℃ 0.018mm Example 2 775℃ 465℃ 418.5℃ 0.02mm

[0079] Conclusion: In both Examples 1 and 2, alloy powders were prepared by vacuum melting and atomization, and the melting points of the prepared alloy powders were 778°C and 775°C, respectively. The alloy powders were mixed with titanium powder and then molded, sintered, and hot-rolled. The sintering temperatures were calculated to be 467°C and 465°C according to the melting point of the alloy powders, and the hot-rolling blanking temperatures were calculated to be 420°C and 418.5°C according to the sintering temperatures. Both the sintering temperature and the hot-rolling blanking temperature were lower than the temperature of the traditional process (600°C), which effectively avoided the reaction of titanium with silver, copper, gold, and tin elements to produce brittle intermetallic compounds, achieved the densification of the alloy powder and the titanium powder alloy blank, and no defects such as brittle fracture and cracking would occur after multiple deformation processes. The thickness of the solder foil prepared in Example 1 was 0.018 mm, and the thickness of the solder foil prepared in Example 2 was 0.02 mm, and both thicknesses were ≤0.02 mm.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification made to the present invention by those skilled in the art without departing from the spirit of the present invention shall fall within the protection scope of the present invention.

Claims

1. A method for preparing a silver-based active solder foil, It is characterized in that The following steps are involved: 1) Preparation of pre-alloyed powder: Silver and one or more elements of copper, gold, tin, lead and indium are vacuum melted and atomized to prepare spherical or quasi-spherical alloy powders; 2) Melting point test: Test steps 1) obtaining the melting point temperature of the alloy powder; 3) Mixing: In an argon or helium atmosphere, the alloy powder of step 1) is mixed with titanium powder, wherein the amount of titanium powder added is 1%-5% of the total weight, and metal balls are added during the mixing; The metal balls are made of silver or copper, and the amount of the metal balls added is 20%-40% of the total weight of the alloy powder; 4) Molding: The mixed powder is pressed into shape at a pressure of 80-120Mpa for 30-90s. 5) Sintering: Sintering under vacuum or protective atmosphere, the sintering temperature is 0.6-0.7 times the melting point temperature, the sintering time is 30-60min, and the sintering temperature is calculated based on the melting point temperature in step 2); 6) Hot rolling Hot rolling to a thickness of 0.2-0.5 mm, the hot rolling blanking temperature is 0.8-0.9 times the sintering temperature, and the hot rolling blanking temperature is calculated based on the sintering temperature in step 5); 7) Surface treatment: The hot-rolled blank is polished and ground to remove impurities such as surface oxide scale; 8) Cold rolling and annealing: The surface treated blank is subjected to multiple cold rolling passes, and annealing treatment is performed after every 4-6 passes. After cold rolling to the target size, annealing treatment is performed again.

2. The preparation method according to claim 1, It is characterized in that Step 1) The vacuum melting temperature is 900-1200°C and the vacuum degree is 1×10 -1 Pa, the vacuum degree of atomization is 1-10Pa, and the gas pressure of atomization is 3-7Mpa.

3. The preparation method according to claim 1, It is characterized in that Step 3) The alloy powder and titanium powder are placed in a silver alloy or copper alloy tank for mixing.

4. The preparation method according to claim 1 or 3, It is characterized in that The alloy powder has a particle size of 5-30 μm, and the titanium powder is spherical or quasi-spherical, has a purity of 99.9%, and a particle size of 5-30 μm.

5. The preparation method according to claim 1, It is characterized in that Step 3) The mixing speed is 10-60r / min and the mixing time is 6-12h.

6. The preparation method according to claim 1, It is characterized in that Step 6) The deformation amount of each hot rolling pass is 30-40%.

7. The preparation method according to claim 1, It is characterized in that Step 8) The deformation amount of each cold rolling pass is 10%-20%.

8. The preparation method according to claim 1, It is characterized in that Step 8) The annealing treatment is performed at a temperature of 300-400°C and for 30 minutes.

Citation Information

Patent Citations

  • Preparation method of ultrathin Ta-W alloy foil

    CN103084388A

  • Preparation method of silver-based flaky electric contact material high in stannic oxide content

    CN105200262A