A modified emulsified asphalt based on SBS and preparation method thereof
By first separating emulsified SBS particles and basic asphalt, and introducing modified nano-attapulgite rods and modified SBS, combined with the process of emulsification first and then modification, the problem of high viscosity and difficulty in balancing the introduction of SBS in modified emulsified asphalt is solved, which is significant. Improved stability and mechanical properties.
Patent Information
- Application Number
- CN202410392126.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-04-02
AI Technical Summary
Existing modified emulsified asphalt has difficulties in balancing between high viscosity and the amount of SBS introduced, resulting in low stability and insufficient cohesion. The adhesion and mechanical strength need to be further improved.
The emulsified SBS particles and base asphalt are first separated and then mixed to improve stability and compatibility. The emulsifier formula is optimized through compound emulsifiers A and B. Modified nano-attapulgite and modified SBS are introduced, combined with emulsification first and then Modified process to improve adhesion and mechanical properties.
It significantly improves the stability, adhesion and mechanical properties of modified emulsified asphalt, enhances fatigue resistance and rutting resistance, and has high applicability.
Smart Images

Figure BDA0004772772870000101 
Figure BDA0004772772870000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road engineering, and in particular to a modified emulsified asphalt based on SBS and a preparation method thereof. Background Art
[0002] With the development of my country's infrastructure industry, the number of highway facilities has increased, which has made highway maintenance more and more important. Among them, emulsified asphalt, as an important material for road construction, has excellent bonding ability, construction convenience, environmental friendliness and other limited features, and is widely used in highway construction and maintenance.
[0003] Modified emulsified asphalt is an advanced material based on emulsified asphalt, which has the dual advantages of modified asphalt and emulsified asphalt. Common modified emulsified asphalt is prepared by SBS modification. In the preparation method, there is either high viscosity, resulting in a low amount of SBS introduced; or there is a balance stability between SBS and asphalt, resulting in low storage stability. Therefore, the type and amount of emulsifier introduced are very important. On the other hand, SBS-modified emulsified asphalt still faces the problem of insufficient cohesion, and the adhesion and mechanical strength still need to be further improved.
[0004] In summary, solving the above problems and preparing a modified emulsified asphalt based on SBS is of great value. Summary of the invention
[0005] The object of the present invention is to provide a modified emulsified asphalt based on SBS and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing a modified emulsified asphalt based on SBS comprises the following steps:
[0008] Step 1: (1) Add compound emulsifier A to deionized water, stir evenly, adjust pH to 2-3, add stabilizer, homogenize, and keep warm at 60-65°C to obtain soap solution B; (2) Heat the base asphalt to 120-140°C, add mercapto polyethylene glycol amino, and homogenize; add it to the preheated colloid mill, add soap solution B, circulate through the mill for 1-3 minutes, and shear for 2-5 minutes to obtain emulsified asphalt;
[0009] Step 2: (1) SBS particles are swollen in a composite solvent and kept warm at 55-60° C. to obtain an SBS solution; (2) a composite emulsifier B and a stabilizer are added to deionized water, homogenized, and kept warm at 55-60° C. to obtain a soap solution A; (3) the SBS solution and the soap solution A are sequentially added to a preheated emulsifier, sheared, rotary evaporated, deionized water added, sheared and homogenized to obtain an SBS latex with a solid content of 20-22 wt %;
[0010] Step 3: Mix SBS latex and emulsified asphalt, and homogenize them to obtain modified emulsified asphalt.
[0011] More optimally, the raw materials of the emulsified asphalt include the following components: by weight, 60 parts of base asphalt, 0.4-0.6 parts of mercapto polyethylene glycol amino, 2.5-3 parts of compound emulsifier A, 0.21-0.42 parts of stabilizer, and 100 parts of deionized water;
[0012] The raw materials of the SBS latex include the following components: by weight, 20-23 parts of SBS particles, 65-75 parts of composite solvents, 7-10 parts of compound emulsifier B, 0.3-0.6 parts of stabilizer, and 45-55 parts of deionized water.
[0013] More optimally, the compound emulsifier A comprises modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:(1-1.5);
[0014] The compound emulsifier B comprises modified SBS, hexadecyltrimethylammonium bromide and nonylphenol polyoxyethylene ether in a mass ratio of (4-6):(1-1.2):(2-2.8).
[0015] More optimally, the preparation method of the modified nano-attapulgite is: adding nano-attapulgite and 4-hexadecylbenzylamine in a mass ratio of 5:1 to DMF in sequence, grinding at 400-500 r / min for 10-12 hours, filtering, washing with ethanol, and freeze-drying to obtain the modified attapulgite.
[0016] More optimally, the preparation method of the modified SBS is:
[0017] (1) linear SBS is added to toluene, and hydrogen bromide-acetic acid solution is added dropwise under ice bath, stirred at room temperature for 24 hours, and post-treated to obtain bromo-SBS;
[0018] (2) Bromo SBS, 18-crown ether-6, and sodium azide are sequentially added to tetrahydrofuran, stirred at 50-55° C. for 4-5 days under a nitrogen atmosphere, and post-treated to obtain azido SBS;
[0019] (3) Adding azidated SBS, alkynyl cyclodextrin, and alkynyl quaternary ammonium salt to tetrahydrofuran, adding anhydrous copper sulfate aqueous solution and sodium ascorbate aqueous solution under nitrogen atmosphere, stirring and reacting at 40-50° C. for 20-24 hours, and post-treating to obtain modified SBS.
[0020] More optimally, the raw materials of the modified SBS include the following components: by weight, 10 parts of azidized SBS, 2 to 4 parts of alkynyl cyclodextrin, 3 to 5 parts of alkynyl quaternary ammonium salt, 0.1 to 0.15 parts of anhydrous copper sulfate, and 0.2 to 0.25 parts of sodium ascorbate.
[0021] More optimally, the preparation method of the alkynyl cyclodextrin is: mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin and propargylamine are sequentially added to a deionized water-thionyl chloride mixed solvent, stirred at 50-55° C. for 20-24 hours under a nitrogen atmosphere, and post-treated to obtain alkynyl cyclodextrin;
[0022] The preparation method of the alkynyl quaternary ammonium salt is as follows: (1) adding diethanolamine, 1-bromobutane, potassium carbonate and potassium iodide to acetonitrile in sequence, and refluxing at 82-85° C. for 12 hours under a nitrogen atmosphere, and post-treating to obtain butyl diethanolamine; (2) adding butyl diethanolamine and propyne bromide to ethanol, and refluxing at 78-80° C. for 12 hours, and post-treating to obtain the alkynyl quaternary ammonium salt.
[0023] More optimally, the composite solvent is cyclohexane and methyl ethyl ketone in a mass ratio of 4:1; the stabilizer includes calcium chloride and cellulose in a mass ratio of 2:1.
[0024] More optimally, the SBS latex accounts for 18-22 wt % of the mass of the emulsified asphalt.
[0025] More optimally, a modified emulsified asphalt with a belt is prepared by a preparation method of modified emulsified asphalt based on SBS.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] In the scheme, in order to overcome the problem between the high viscosity of the modified emulsified asphalt and the amount of SBS introduced, the SBS particles and the base asphalt are first emulsified separately, and then the obtained SBS latex and emulsified asphalt are mixed, so as to improve the stability and compatibility of the modified emulsified asphalt in a way of emulsification first and then modification.
[0028] In the scheme, compound emulsifier A and compound emulsifier B with different formulas are used to emulsify base asphalt and SBS latex, thereby improving the adhesion, mechanical properties and fatigue resistance of the modified emulsified asphalt on the basis of achieving optimal emulsification and stability.
[0029] First, the compound emulsifier A is compounded with modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether; it is used to pre-emulsify the base asphalt, wherein the modified nano-attapulgite is based on the nano-attapulgite and is obtained by grinding and modifying it with 4-hexadecylbenzylamine; the nano-attapulgite is a nano-material with a fibrous structure and has adsorption properties. Its introduction can improve the interface between asphalt and the emulsifier. At the same time, 4-hexadecylbenzylamine is used in advance to make the modified nano-attapulgite have a viscosity-reducing property, improve the permeability and mixing of the emulsifier, and have affinity with the cationic emulsifier hexadecyltrimethylammonium bromide, thereby further enhancing the emulsification and stability. At the same time, its introduction can improve the mechanical properties and increase the anti-rutting performance.
[0030] Compared with a single emulsifier, the cationic hexadecyltrimethylammonium bromide and nonionic nonylphenol polyoxyethylene ether compounded with modified nano-attapulgite have good dispersibility and electrochemical stability, and can effectively disperse asphalt in the water phase to form a stable emulsion, while the nonionic emulsifier can increase the compatibility between the emulsifier and asphalt. Synergy can achieve better performance, but it should be noted that the ratio needs to be limited, because too much cationic emulsifier will cause the emulsifier to aggregate and reduce the emulsification effect.
[0031] Secondly, the SBS granular emulsifier is emulsified using a compound emulsifier B, which also includes hexadecyltrimethylammonium bromide and nonylphenol polyoxyethylene ether; in addition, it also includes modified SBS, which is used to increase the cohesion of the modified emulsified asphalt while ensuring stability, thereby increasing adhesion and mechanical properties.
[0032] Among them, due to the special structure of SBS, in order to improve the stability of SBS modified emulsified asphalt, a modified SBS is introduced, which is based on straight-chain SBS, and is successively brominated and azidized, and then the reaction between the azide group and the alkynyl group is used to graft alkynyl cyclodextrin and alkynyl quaternary ammonium salt; since it has similar chain segments with SBS, its introduction can improve the interface between the emulsifier and the SBS particles, thereby improving the emulsification and stability. On the other hand, the grafted cyclodextrin can improve the cohesion, improve the flexibility, adhesion and durability of the emulsified asphalt, but too much grafting will increase the viscosity and reduce the stability; therefore, the scheme further introduces the grafting of alkynyl quaternary ammonium salt, which can promote the emulsification of cationic hexadecyl trimethyl ammonium bromide and nonylphenol polyoxyethylene ether, and can enhance the interaction and cohesion between asphalt, thereby improving the stability and adhesion of the modified emulsified asphalt. In addition, since it is azidated before grafting, it contains nitrogen-containing rings, which can improve the compatibility with asphalt, improve the stability of emulsified asphalt, and make the modified emulsified asphalt have corrosion inhibition. It should be noted that the ratio needs to be limited, because the introduction of too much modified SBS will lead to increased viscosity and decreased stability. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are exemplified without any special restrictions: in the following embodiments, parts are by mass; linear SBS is SBS TSRC 4270 low molecular weight linear copolymer, model D-KX410CS, brand Keteng TSRC; SBS particles are star-shaped SBS4303, brand Yanshan Petrochemical; matrix asphalt is SK-90# asphalt; the molecular weight of mercapto polyethylene glycol amino is 600, brand Xi'an Kaixin Biology; the specification of calcium chloride is analytical grade, brand is Sinopharm Reagent; the specification of cellulose is analytical grade, brand is Sinopharm Reagent; the CAS number of hexadecyltrimethylammonium bromide is 57-09-0, and the CAS number of nonylphenol polyoxyethylene ether is 9016-45-9; the CAS number of propargylamine is 2450-71-7; the CAS number of diethanolamine is 111-42-2; the average fineness of nano-attapulgite is 30nm; the above raw materials and the remaining raw materials are all commercially available.
[0035] (1) Preparation of modified attapulgite: 5 parts of nano-attapulgite and 1 part of 4-hexadecylbenzylamine were added to 30 parts of DMF in sequence, ground at 500 r / min for 10 hours, filtered, washed with ethanol, and freeze-dried to obtain modified attapulgite;
[0036] (2) Preparation of alkynyl cyclodextrin: 1 part of mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin and 1.5 parts of propargylamine were added to 50 parts of a deionized water-thionyl chloride mixed solvent (the mass ratio of deionized water to thionyl chloride was 1:1) in sequence, and stirred at 50° C. for 24 hours under a nitrogen atmosphere, and post-treated to obtain alkynyl cyclodextrin;
[0037] (3) Preparation of alkynyl quaternary ammonium salt: 4.5 parts of diethanolamine, 4.8 parts of 1-bromobutane, 8.2 parts of potassium carbonate and 1 part of potassium iodide were added to 80 parts of acetonitrile in sequence, and refluxed at 82° C. for 12 hours under a nitrogen atmosphere, and post-treated to obtain butyl diethanolamine; 3.2 parts of butyl diethanolamine and 3.1 parts of bromopropyne were added to 100 parts of ethanol, refluxed at 80° C. for 12 hours, and post-treated to obtain alkynyl quaternary ammonium salt;
[0038] (4) Preparation of SBS azidate: 1 part of linear SBS was added to 60 parts of toluene, and a hydrogen bromide-acetic acid solution (1.5 parts of hydrogen bromide and 20 parts of acetic acid) was added dropwise under an ice bath, and stirred at room temperature for 24 hours, and post-treated to obtain bromo SBS; 1.5 parts of bromo SBS, 0.25 parts of 18-crown ether-6, and 3 parts of sodium azide were added to 60 parts of tetrahydrofuran in sequence, and stirred at 50° C. for 5 days under a nitrogen atmosphere, and post-treated to obtain SBS azidate;
[0039] Example 1: A method for preparing a modified emulsified asphalt based on SBS, comprising the following steps:
[0040] Pre-preparation: 10 parts of azidated SBS, 3 parts of alkynyl cyclodextrin, and 4 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50° C. for 24 hours, and post-treated to obtain modified SBS;
[0041] Step 1: (1) Add 3 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.3, add 0.3 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.5 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0042] Step 2: (1) 22 parts of SBS particles were swollen in 70 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 8 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 5:1:2) and 0.42 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. Homogenize and keep warm at 60°C to obtain soap solution A; (3) add the SBS solution and soap solution A to a preheated emulsifier in sequence, shear at 800 r / min for 1 minute, shear at 1500 r / min for 5 minutes, and shear at 3000 r / min for 5 minutes, remove the complex solvent by rotary evaporation at 50°C and -0.1 MPa vacuum, add deionized water, and shear and homogenize at 800 r / min to obtain an SBS latex with a solid content of 20 wt%;
[0043] Step 3: Mix SBS latex and emulsified asphalt (SBS latex accounts for 20wt% of the mass of emulsified asphalt), homogenize, and obtain modified emulsified asphalt.
[0044] Embodiment 2: A method for preparing a modified emulsified asphalt based on SBS, comprising the following steps:
[0045] Pre-preparation: 10 parts of azidated SBS, 3 parts of alkynyl cyclodextrin, and 5 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50° C. for 24 hours, and post-treated to obtain modified SBS;
[0046] Step 1: (1) Add 2.5 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1) to 100 parts of deionized water, stir evenly, adjust the pH to 2.6, add 0.21 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 65°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.6 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0047] Step 2: (1) 23 parts of SBS particles were swollen in 75 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 10 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 6:1.2:2.8) and 0.6 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water and the mixture was heated at 500 r / min. n, and keep warm at 60° C. to obtain soap solution A; (3) adding the SBS solution and soap solution A to a preheated emulsifier in sequence, shearing at 800 r / min for 1 minute, shearing at 1500 r / min for 5 minutes, and shearing at 3000 r / min for 5 minutes, removing the composite solvent by rotary evaporation at 50° C. and a vacuum degree of −0.1 MPa, adding deionized water, and shearing and homogenizing at 800 r / min to obtain an SBS latex with a solid content of 20 wt %;
[0048] Step 3: SBS latex and emulsified asphalt are mixed (SBS latex accounts for 18 wt% of the mass of emulsified asphalt), and homogenized to obtain modified emulsified asphalt.
[0049] Embodiment 3: A method for preparing a modified emulsified asphalt based on SBS, comprising the following steps:
[0050] Pre-preparation: 10 parts of azidated SBS, 3 parts of alkynyl cyclodextrin, and 3 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50°C for 24 hours, and post-treated to obtain modified SBS;
[0051] Step 1: (1) Add 3 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.5, add 0.42 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 120°C, add 0.4 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0052] Step 2: (1) 20 parts of SBS particles were swollen in 65 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 55°C to obtain an SBS solution; (2) 7 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 4:1:2) and 0.3 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. Homogenize and keep warm at 55°C to obtain soap solution A; (3) add the SBS solution and soap solution A to a preheated emulsifier in sequence, shear at 800 r / min for 1 minute, shear at 1500 r / min for 5 minutes, and shear at 3000 r / min for 5 minutes, remove the complex solvent by rotary evaporation at 50°C and -0.1 MPa vacuum, add deionized water, and shear and homogenize at 800 r / min to obtain an SBS latex with a solid content of 20 wt%;
[0053] Step 3: SBS latex and emulsified asphalt are mixed (SBS latex accounts for 22 wt% of the mass of emulsified asphalt), and homogenized to obtain modified emulsified asphalt.
[0054] Comparative Example 1: Linear SBS, alkynyl cyclodextrin, and alkynyl quaternary ammonium salt are used instead of modified SBS, and the rest is the same as Example 1; comprising the following steps:
[0055] Pre-preparation: 3 parts of linear SBS, 0.8 parts of alkynyl cyclodextrin, and 1.2 parts of alkynyl quaternary ammonium salt were mixed to obtain a complex;
[0056] Step 1: (1) Add 3 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.3, add 0.3 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.5 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0057] Step 2: (1) 22 parts of SBS particles were swollen in 70 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 8 parts of a composite emulsifier B (a composite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 5:1:2) and 0.42 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. (3) adding the SBS solution and the soap solution A to a preheated emulsifier in sequence, shearing at 800 r / min for 1 minute, shearing at 1500 r / min for 5 minutes, and shearing at 3000 r / min for 5 minutes, removing the composite solvent by rotary evaporation at 50°C and a vacuum degree of -0.1 MPa, adding deionized water, and shearing and homogenizing at 800 r / min to obtain an SBS latex with a solid content of 20 wt%;
[0058] Step 3: Mix SBS latex and emulsified asphalt (SBS latex accounts for 20wt% of the mass of emulsified asphalt), homogenize, and obtain modified emulsified asphalt.
[0059] Comparative Example 2: In the modified SBS, alkynyl cyclodextrin is not grafted, and the rest is the same as Example 1, comprising the following steps:
[0060] Pre-preparation: 10 parts of azidized SBS and 7 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50°C for 24 hours, and post-treated to obtain modified SBS;
[0061] Step 1: (1) Add 3 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.3, add 0.3 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.5 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0062] Step 2: (1) 22 parts of SBS particles were swollen in 70 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 8 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 5:1:2) and 0.42 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. Homogenize and keep warm at 60°C to obtain soap solution A; (3) add the SBS solution and soap solution A to a preheated emulsifier in sequence, shear at 800 r / min for 1 minute, shear at 1500 r / min for 5 minutes, and shear at 3000 r / min for 5 minutes, remove the complex solvent by rotary evaporation at 50°C and -0.1 MPa vacuum, add deionized water, and shear and homogenize at 800 r / min to obtain an SBS latex with a solid content of 20 wt%;
[0063] Step 3: Mix SBS latex and emulsified asphalt (SBS latex accounts for 20wt% of the mass of emulsified asphalt), homogenize, and obtain modified emulsified asphalt.
[0064] Comparative Example 3: Increasing the amount of modified SBS introduced, the rest is the same as Example 1, comprising the following steps:
[0065] Pre-preparation: 10 parts of azidated SBS, 3 parts of alkynyl cyclodextrin, and 4 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50° C. for 24 hours, and post-treated to obtain modified SBS;
[0066] Step 1: (1) Add 3 parts of compound emulsifier A (modified nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.3, add 0.3 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.5 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0067] Step 2: (1) 22 parts of SBS particles were swollen in 70 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 12 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 9:1:2) and 0.42 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. (3) adding the SBS solution and the soap solution A to a preheated emulsifier in sequence, shearing at 800 r / min for 1 minute, shearing at 1500 r / min for 5 minutes, and shearing at 3000 r / min for 5 minutes, removing the composite solvent by rotary evaporation at 50° C. and a vacuum degree of −0.1 MPa, adding deionized water, and shearing and homogenizing at 800 r / min to obtain an SBS latex with a solid content of 20 wt %;
[0068] Step 3: Mix SBS latex and emulsified asphalt (SBS latex accounts for 20wt% of the mass of emulsified asphalt), homogenize, and obtain modified emulsified asphalt.
[0069] Comparative Example 4: The modified attapulgite is replaced by attapulgite, and the rest is the same as Example 1; comprising the following steps:
[0070] Pre-preparation: 10 parts of azidated SBS, 3 parts of alkynyl cyclodextrin, and 4 parts of alkynyl quaternary ammonium salt were added to tetrahydrofuran, and under a nitrogen atmosphere, anhydrous copper sulfate aqueous solution (0.12 parts of anhydrous copper sulfate, 10 parts of deionized water) and sodium ascorbate aqueous solution (0.24 parts of sodium ascorbate, 10 parts of deionized water) were added, and the mixture was stirred at 50° C. for 24 hours, and post-treated to obtain modified SBS;
[0071] Step 1: (1) Add 3 parts of compound emulsifier A (nano-attapulgite, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:1.5) to 100 parts of deionized water, stir evenly, adjust the pH to 2.3, add 0.3 parts of stabilizer (calcium chloride and cellulose in a mass ratio of 2:1), homogenize at 500 r / min, and keep warm at 60°C to obtain soap solution B; (2) Heat 60 parts of base asphalt to 140°C, add 0.5 parts of mercapto polyethylene glycol amino, and homogenize at 3000 r / min; add it to a preheated colloid mill, add soap solution B, circulate through the mill for 2 minutes, and shear at 800 r / min for 3 minutes to obtain emulsified asphalt;
[0072] Step 2: (1) 22 parts of SBS particles were swollen in 70 parts of a composite solvent (cyclohexane and methyl ethyl ketone in a mass ratio of 4:1), and the mixture was kept warm at 60°C to obtain an SBS solution; (2) 8 parts of a composite emulsifier B (modified SBS, hexadecyltrimethylammonium bromide, and nonylphenol polyoxyethylene ether in a mass ratio of 5:1:2) and 0.42 parts of a stabilizer (calcium chloride and cellulose in a mass ratio of 2:1) were added to 50 parts of deionized water, and the mixture was stirred at 500 r / min. Homogenize and keep warm at 60°C to obtain soap solution A; (3) add the SBS solution and soap solution A to a preheated emulsifier in sequence, shear at 800 r / min for 1 minute, shear at 1500 r / min for 5 minutes, and shear at 3000 r / min for 5 minutes, remove the complex solvent by rotary evaporation at 50°C and -0.1 MPa vacuum, add deionized water, and shear and homogenize at 800 r / min to obtain an SBS latex with a solid content of 20 wt%;
[0073] Step 3: Mix SBS latex and emulsified asphalt (SBS latex accounts for 20wt% of the mass of emulsified asphalt), homogenize, and obtain modified emulsified asphalt.
[0074] Performance test 1: (1) Test its storage stability according to JTG E20-2011 "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering". (2) Take 500g of 19mm, 7.5g of modified emulsified asphalt evaporation residue, and 500g of 16mm aggregate, keep them at 165℃ for 2 hours, then mix them in sequence and cool them at room temperature; test and calculate the anti-stripping degree; (3) Place the modified emulsified asphalt evaporation residue in a mixed soil block, combine and shape it, place it at room temperature for 1 hour, and test the pull-out performance at a rate of 10mm / min; the obtained data are shown in the following table:
[0075] Storage stability 5d (%) Anti-stripping degree (%) Tensile strength (MPa) Example 1 1.53 53.03 1.61 Example 2 1.56 51.78 1.57 Example 3 1.58 52.23 1.58 Comparative Example 1 1.83 47.77 1.35 Comparative Example 2 1.62 48.84 1.44 Comparative Example 3 1.66 49.85 1.47 Comparative Example 4 1.60 50.91 1.52
[0076] Conclusion: The present invention discloses a modified emulsified asphalt based on SBS and a preparation method thereof. The process design is reasonable. By introducing modified attapulgite and modified SBS into the compound emulsifiers A and B, combined with a process of emulsification followed by modification, the final modified emulsified asphalt has excellent stability, adhesion and mechanical strength and is highly applicable.
[0077] Performance Test 2: The basic properties of the modified emulsified asphalt obtained in Example 1 were tested, and the obtained data were as follows:
[0078]
[0079]
[0080] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a modified emulsified asphalt based on SBS, characterized in that: The following steps are involved: Step 1: (1) Add compound emulsifier A to deionized water, stir evenly, adjust pH to 2-3, add stabilizer, homogenize, and keep warm at 60-65°C to obtain soap solution B; (2) Heat the base asphalt to 120-140°C, add mercapto polyethylene glycol amino, and homogenize; add it to the preheated colloid mill, add soap solution B, circulate through the mill for 1-3 minutes, and shear for 2-5 minutes to obtain emulsified asphalt; Step 2: (1) SBS particles are swollen in a composite solvent and kept warm at 55-60° C. to obtain an SBS solution; (2) a composite emulsifier B and a stabilizer are added to deionized water, homogenized, and kept warm at 55-60° C. to obtain a soap solution A; (3) the SBS solution and the soap solution A are sequentially added to a preheated emulsifier, sheared, rotary evaporated, deionized water added, sheared and homogenized to obtain an SBS latex with a solid content of 20-22 wt %; Step 3: Mix the SBS latex and the emulsified asphalt, and homogenize them to obtain modified emulsified asphalt; The raw materials of the emulsified asphalt include the following components: by weight, 60 parts of base asphalt, 0.4-0.6 parts of mercapto polyethylene glycol amino, 2.5-3 parts of compound emulsifier A, 0.21-0.42 parts of stabilizer, and 100 parts of deionized water; The raw materials of the SBS latex include the following components: by weight, 20 to 23 parts of SBS particles, 65 to 75 parts of composite solvent, 7 to 10 parts of composite emulsifier B, 0.3 to 0.6 parts of stabilizer, and 45 to 55 parts of deionized water; The compound emulsifier A comprises modified nano-attapulgite, hexadecyltrimethylammonium bromide and nonylphenol polyoxyethylene ether in a mass ratio of 0.5:1:(1-1.5); The compound emulsifier B comprises modified SBS, hexadecyltrimethylammonium bromide and nonylphenol polyoxyethylene ether in a mass ratio of (4-6):(1-1.2):(2-2.8); The preparation method of the modified nano attapulgite is as follows: adding nano attapulgite and 4-hexadecylbenzylamine in a mass ratio of 5:1 to DMF in sequence, grinding at 400-500 r / min for 10-12 hours, filtering, washing with ethanol, and freeze-drying to obtain the modified attapulgite; The preparation method of the modified SBS is as follows: (1) adding linear SBS to toluene, adding hydrogen bromide-acetic acid solution dropwise under ice bath, stirring at room temperature for 24 hours, post-treating to obtain bromo SBS; (2) adding bromo SBS, 18-crown ether-6, and sodium azide to tetrahydrofuran in sequence, stirring and reacting at 50-55° C. for 4-5 days under nitrogen atmosphere, post-treating to obtain azid SBS; (3) adding azid SBS, alkynyl cyclodextrin, and alkynyl quaternary ammonium salt to tetrahydrofuran, adding anhydrous copper sulfate aqueous solution and sodium ascorbate aqueous solution under nitrogen atmosphere, stirring and reacting at 40-50° C. for 20-24 hours, post-treating to obtain modified SBS.
2. The method for preparing a modified emulsified asphalt based on SBS according to claim 1, characterized in that: The raw materials of the modified SBS include the following components: by weight, 10 parts of azidized SBS, 2-4 parts of alkynyl cyclodextrin, 3-5 parts of alkynyl quaternary ammonium salt, 0.1-0.15 parts of anhydrous copper sulfate, and 0.2-0.25 parts of sodium ascorbate.
3. The method for preparing a modified emulsified asphalt based on SBS according to claim 1, characterized in that: The preparation method of the alkynyl cyclodextrin is as follows: mono-6-O-(p-toluenesulfonyl)-β-cyclodextrin and propargylamine are sequentially added to a deionized water-thionyl chloride mixed solvent, stirred at 50-55° C. for 20-24 hours under a nitrogen atmosphere, and post-treated to obtain alkynyl cyclodextrin; The preparation method of the alkynyl quaternary ammonium salt is as follows: (1) adding diethanolamine, 1-bromobutane, potassium carbonate and potassium iodide to acetonitrile in sequence, and refluxing at 82-85° C. for 12 hours under a nitrogen atmosphere, and post-treating to obtain butyl diethanolamine; (2) adding butyl diethanolamine and propyne bromide to ethanol, and refluxing at 78-80° C. for 12 hours, and post-treating to obtain the alkynyl quaternary ammonium salt.
4. The method for preparing a modified emulsified asphalt based on SBS according to claim 1, characterized in that: The composite solvent comprises cyclohexane and methyl ethyl ketone in a mass ratio of 4:1; and the stabilizer comprises calcium chloride and cellulose in a mass ratio of 2:
1.
5. The method for preparing a modified emulsified asphalt based on SBS according to claim 1, characterized in that: The SBS latex accounts for 18-22 wt % of the mass of the emulsified asphalt.
6. The modified emulsified asphalt prepared according to the method for preparing a modified emulsified asphalt based on SBS according to any one of claims 1 to 5.
Citation Information
Patent Citations
SBS (styrene-butadiene-styrene) modified emulsified asphalt composition and preparation method thereof
CN102120889A
Efficient SBS (styrene-butadiene-styrene) modified asphalt stabilizer
CN104927388A
SBS latex modified emulsified asphalt and preparation method and application thereof
CN105219270A
Ultrathin road wearing layer and construction method thereof
CN116145492A
Modified asphalt composite material, preparation method and application of modified asphalt composite material in ultrathin wearing layer
CN117303800A