Putty for light alloy and preparation method thereof

Through the formulation of two-component multifunctional light putty, using styrene, dicyclopentadiene resin and specific surfactants, the problems of slow curing rate and poor coloring performance of sheet metal ash are solved, and rapid curing and efficient coloring are achieved. Improve construction efficiency and storage stability.

CN118290981BActive Publication Date: 2024-11-08GUANGZHOU ZHONGHAN CHUANGNENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410542390.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-08
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The existing sheet metal gray has slow curing rate, poor tint intensity, low gloss and low color durability.

Method used

Adopt a two-component multi-function light putty formula, including component A and component B. Component A contains styrene, dicyclopentadiene resin, dispersant, defoaming agent, wetting agent, anti-rust agent, zinc phosphate Anti-rust pigment, aniline black and silicone surfactant. Component B consists of benzoyl peroxide and tert-butyl neodecanoate peroxide. The mass ratio of component A to component B is 100: (1.5~3 ) and carboxylate type bimini surfactants and silicone surfactants are used to improve curing efficiency and coloring properties.

Benefits of technology

It realizes the fast curing, strong adhesion, good coloring strength and gloss of putty, and has high storage stability and construction efficiency, and is low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004821323550000051
    Figure BDA0004821323550000051
  • Figure BDA0004821323550000061
    Figure BDA0004821323550000061
  • Figure BDA0004821323550000062
    Figure BDA0004821323550000062
Patent Text Reader

Abstract

The invention belongs to the technical field of sheet metal ash, and relates to a putty for light alloy and a preparation method thereof. The putty comprises the following components: composed of component A and component B, wherein component A comprises: styrene, dicyclopentadiene resin, dispersant, defoamer, wetting agent, rust inhibitor, zinc phosphate rust-proof pigment, aniline black, leveling agent, silicone surfactant, carboxylate type gemini surfactant; and component B comprises the following components: benzoyl peroxide (BPO) and tert-butyl peroxyneodecanoate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sheet metal putty and relates to a putty for light alloy and a preparation method thereof. Background Art

[0002] Sheet metal ash, also known as Poly-PuttyBase, is an unsaturated polyester resin putty. It is an embedding material used for automobile sheet metal repair. It has developed rapidly in the past 20 years and has greatly improved the efficiency and quality of automobile sheet metal repair. The general composition of sheet metal ash includes modified resin, pigment, filler, anti-settling agent, cobalt salt initiator inhibitor and other additives, as well as curing agent (peroxide). After these ingredients are mixed in a certain proportion, they can be quickly dried at room temperature, easy to scrape and polish, have strong adhesion, high heat resistance, good flexibility, and are not easy to crack or blister. The curing agent component used in sheet metal ash is a type of substance or mixture that promotes or controls the curing reaction. Resin curing is a process in which thermosetting resin undergoes irreversible changes through chemical reactions such as condensation, ring closure, addition or catalysis. Curing is achieved by adding a curing (cross-linking) agent. Curing agent is an indispensable additive. Whether it is used as an adhesive, coating, or casting material, curing agent must be added, otherwise the epoxy resin cannot be cured. The type of curing agent has a great influence on the mechanical properties, heat resistance, water resistance, corrosion resistance, etc. of the cured product.

[0003] Based on the above analysis, it is very necessary to provide a method for finding a suitable formula while ensuring the curing efficiency of the putty, so as to keep the putty having high tinting strength, glossiness and stable and durable color. Summary of the invention

[0004] The present application provides a putty for lightweight alloys and a preparation method thereof. The putty is a two-component multifunctional lightweight putty, which has the advantages of fast curing and strong adhesion, is suitable for a variety of metal substrates, and has good adhesion to galvanized sheets. The curing agent has no irritating odor and is very environmentally friendly. The putty has a low specific gravity and is particularly easy to apply, scrape and polish. Compared with heavy putties of the same quality, it has a larger construction area, higher construction efficiency, and lower overall cost. It is an upgraded product of traditional sheet metal ash. The putty for lightweight alloys can solve the technical problems of slow curing rate in the prior art, poor tinting strength of the cured product, low gloss, and low color durability.

[0005] The technical solution of the present invention is:

[0006] Provided is a putty for light alloys, characterized in that it consists of component A and component B, wherein component A comprises the following components in parts by mass: 5-20 parts of styrene, 45-60 parts of dicyclopentadiene resin, 0.5-5 parts of dispersant, 0.1-1 parts of defoamer, 0.1-1 parts of wetting agent, 0.1-1 parts of rust inhibitor, 15-20 parts of zinc phosphate rust-proof pigment, 1-7 parts of aniline black, 1-2 parts of leveling agent, 1-1.5 parts of organosilicon surfactant, and 0.1-0.5 parts of carboxylate gemini surfactant; component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of (0.7-1.5):(0.8-1.5); and the mass ratio of component A to component B is 100:(1.5-3).

[0007] Furthermore, the component A includes the following components in parts by mass: 12.5 parts of styrene, 57 parts of dicyclopentadiene resin, 4 parts of dispersant, 1 part of defoamer, 0.5 part of wetting agent, 0.5 part of rust inhibitor, 16.5 parts of zinc phosphate antirust pigment, 5 parts of aniline black, 1.5 parts of leveling agent, 1 part of silicone surfactant, and 0.5 part of carboxylate type gemini surfactant; the component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.5:1; the mass ratio of component A to component B is 100:2.5.

[0008] Furthermore, the dispersant is a German BYK brand with a model number of BYK190; the defoaming agent is a German Tego brand with a model number of TEGO825; the wetting agent is a German Tego brand with a model number of TEGO254; the rust inhibitor is a Qingdao Enze brand with a model number of anti-flash rust agent CK34; the leveling agent is a German BYK brand with a model number of BYK307; the silicone surfactant product specification is MY1291, which was purchased from Anhui Mingyi Co., Ltd.

[0009] Furthermore, the carboxylate type gemini surfactant is a carboxylate type gemini surfactant CGS-2, which is prepared by the following process: 10g N, N'-didodecylethylenediamine and 7.6g succinic anhydride are dissolved in 50mL tetrahydrofuran, reacted at 70°C for 24h, and after the reaction is completed, the solvent is evaporated under reduced pressure to obtain a white powder solid A, the obtained solid A is dispersed in 100mL deionized water, the pH is adjusted to 10-11 with a NaOH solution, the insoluble matter is filtered out, the filtrate is collected, the pH of the filtrate is adjusted to 1-2 with hydrochloric acid, the insoluble matter is collected, and the solid is washed with distilled water until neutral to obtain a solid B, and then recrystallized 2-3 times with a mixed solvent of ethyl acetate and ethanol, wherein the volume ratio of ethyl acetate to ethanol is 1:3, to obtain a white powder solid C, the obtained solid C is dissolved in an ethanol solution of NaOH, the solvent is evaporated under reduced pressure and the obtained solid D is dispersed in chloroform, the insoluble matter is filtered out, and the carboxylate type gemini surfactant CGS-2 is obtained.

[0010] Furthermore, the zinc phosphate anti-rust pigment was purchased from Jinan Quanxing New Materials Co., Ltd.

[0011] The present invention also provides a method for preparing the above-mentioned putty for light alloy, comprising the following steps:

[0012] S1. First, component A is prepared according to the mass ratio, styrene, dicyclopentadiene resin, silicone surfactant MY1291, carboxylate type gemini surfactant CGS-2, and dispersant BYK190 are first mixed evenly, zinc phosphate antirust pigment and aniline black are added in a dispersed state, and after mixing evenly, the remaining components of component A are added, dispersed and stirred evenly to obtain a uniformly mixed component A, and then component B is prepared according to the mass ratio, benzoyl peroxide and tert-butyl peroxyneodecanoate are added, and stirred evenly to obtain a uniformly mixed component A;

[0013] S2. Before use, mix the uniformly mixed component A and the uniformly mixed component B in the mass ratio.

[0014] The present invention also provides a method for using the above-mentioned putty for light alloy, comprising the following steps: S1, removing oil, rust, old paint film and moisture on the surface of the coating before use, and keeping the surface of the coating clean and dry; S2, evenly blending component A and component B according to a mass ratio of 100: (1.5-3) to obtain a putty with uniform color; S3, applying and scraping the putty obtained in S2 within 15 minutes.

[0015] Furthermore, after step S3, step S4 is also included, and after the coating is completed, dry grinding can be performed after the putty is completely hardened.

[0016] Furthermore, the coating surface in step S1 refers to one or more of a glass fiber reinforced plastic surface, an iron plate surface, a steel plate surface, an aluminum plate surface, and a galvanized plate surface.

[0017] Furthermore, before step S1, the temperature and humidity of the coating environment are measured. If the ambient temperature is greater than or equal to 25 degrees Celsius and the relative humidity is greater than or equal to 70% RH, the coating time in S2 can be extended from within 15 minutes to within 20 minutes.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present application uses a specific surfactant to significantly improve the stability of aniline black in the putty, so that the putty has good storage stability and black glossiness.

[0020] (2) The present application uses two curing agent active ingredients, benzoyl peroxide (BPO) and tert-butyl peroxyneodecanoate, which have a shorter curing time and higher efficiency than monomers of equal mass. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0022] Example 1

[0023] A putty for light alloy

[0024] Reference Table 1 for the recipe of this embodiment

[0025] Table 1 Recipe

[0026] Component A Dosage wt% Dicyclopentadiene resin 57 Styrene 12.5 Dispersant BYK190 4 Defoamer TEGO825 1 Wetting agent TEGO254 0.5 Rust inhibitor CK34 0.5 Leveling agent BYK307 1.5 Zinc phosphate anti-rust pigment 16.5 Aniline Black 5 Silicone surfactant MY1291 1 Carboxylate Gemini Surfactant CGS-2 0.5

[0027] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.5:1.

[0028] The mass ratio of component A to component B is 100:2.5.

[0029] The carboxylate type Gemini surfactant is a carboxylate type Gemini surfactant CGS-2, which is prepared by the following process: 10g N, N'-didodecylethylenediamine and 7.6g succinic anhydride are dissolved in 50mL tetrahydrofuran, reacted at 70°C for 24h, and after the reaction is completed, the solvent is evaporated under reduced pressure to obtain a white powder solid A, the obtained solid A is dispersed in 100mL deionized water, the pH is adjusted to 10 with a NaOH solution, the insoluble matter is filtered out, the filtrate is collected, the pH of the filtrate is adjusted to 2 with hydrochloric acid, the insoluble matter is collected, and the solid B is washed with distilled water until neutral to obtain a solid B, and then recrystallized twice with a mixed solvent of ethyl acetate and ethanol, wherein the volume ratio of ethyl acetate to ethanol is 1:3, to obtain a white powder solid C, the obtained solid C is dissolved in an ethanol solution of NaOH, the solvent is evaporated under reduced pressure, and the obtained solid D is dispersed in chloroform, the insoluble matter is filtered out, and the carboxylate type Gemini surfactant CGS-2 is obtained by evaporating the solvent.

[0030] The zinc phosphate anti-rust pigment was purchased from Jinan Quanxing New Materials Co., Ltd.

[0031] The method for preparing the putty for light alloy comprises the following steps:

[0032] S1. First, component A is prepared according to the mass ratio, styrene, dicyclopentadiene resin, silicone surfactant MY1291, carboxylate type gemini surfactant CGS-2, and dispersant BYK190 are first mixed evenly, zinc phosphate antirust pigment and aniline black are added in a dispersed state, and after mixing evenly, the remaining components of component A are added, dispersed and stirred evenly to obtain a uniformly mixed component A, and then component B is prepared according to the mass ratio, benzoyl peroxide and tert-butyl peroxyneodecanoate are added, and stirred evenly to obtain a uniformly mixed component A;

[0033] S2. Before use, mix the uniformly mixed component A and the uniformly mixed component B in the mass ratio.

[0034] Example 2

[0035] The formula of this embodiment 2 refers to Table 2, and the preparation method of this embodiment is the same as that of embodiment 1.

[0036] Table 2 Recipe

[0037]

[0038]

[0039] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.4:1.1.

[0040] The mass ratio of component A to component B is 100:2.5.

[0041] Example 3

[0042] The formula of this embodiment 3 refers to Table 3, and the preparation method of this embodiment is the same as that of embodiment 1.

[0043] Table 3 Recipe

[0044] Component A Dosage wt% Dicyclopentadiene resin 60 Styrene 10 Dispersant BYK190 4 Defoamer TEGO825 1.9 Wetting agent TEGO254 0.8 Rust inhibitor CK34 0.7 Leveling agent BYK307 1.3 Zinc phosphate anti-rust pigment 14.6 Aniline Black 4.9 Silicone surfactant MY1291 1.5 Carboxylate Gemini Surfactant CGS-2 0.3

[0045] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.3:1.2.

[0046] The mass ratio of component A to component B is 100:2.5.

[0047] Comparative Example 1

[0048] The formula of this comparative example 1 refers to Table 4, and the preparation method of this comparative example is the same as that of Example 1.

[0049] Table 4 Recipe

[0050]

[0051]

[0052] The component B consists only of benzoyl peroxide.

[0053] The mass ratio of component A to component B is 100:2.5.

[0054] Comparative Example 2

[0055] The formula of this comparative example 2 is referred to Table 5, and the preparation method of this comparative example is the same as that of Example 1

[0056] Table 5 Recipe

[0057] Component A Dosage wt% Dicyclopentadiene resin 57 Styrene 12.5 Dispersant BYK190 4 Defoamer TEGO825 1 Wetting agent TEGO254 0.5 Rust inhibitor CK34 0.5 Leveling agent BYK307 1.5 Zinc phosphate anti-rust pigment 16.5 Aniline Black 5 Silicone surfactant MY1291 1 Carboxylate Gemini Surfactant CGS-2 0.5

[0058] The component B consists only of tert-butyl ammonium peroxyneodecanoate.

[0059] The mass ratio of component A to component B is 100:2.5.

[0060] Comparative Example 3

[0061] The formula of this comparative example 3 is referred to Table 6, and the preparation method of this comparative example is the same as that of Example 1

[0062] Table 6 Recipe

[0063]

[0064]

[0065] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.4:1.1.

[0066] The mass ratio of component A to component B is 100:2.5.

[0067] Comparative Example 4

[0068] The formula of this comparative example 4 is referred to Table 7, and the preparation method of this comparative example is the same as that of Example 1

[0069] Table 7 Recipe

[0070] Component A Dosage wt% Dicyclopentadiene resin 60 Styrene 10 Dispersant BYK190 4 Defoamer TEGO825 1.9 Wetting agent TEGO254 0.8 Rust inhibitor CK34 0.7 Leveling agent BYK307 1.3 Zinc phosphate anti-rust pigment 14.6 Aniline Black 4.9 Silicone surfactant MY1291 1.8 Carboxylate Gemini Surfactant CGS-2 0

[0071] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.3:1.2.

[0072] The mass ratio of component A to component B is 100:2.5.

[0073] Comparative Example 5

[0074] The formula of this comparative example 5 is referred to Table 8, and the preparation method of this comparative example is the same as that of Example 1

[0075] Table 8 Recipe

[0076]

[0077]

[0078] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.3:1.2.

[0079] The mass ratio of component A to component B is 100:2.5.

[0080] Comparative Example 6

[0081] The formula of this comparative example 6 refers to Table 9, and the preparation method of this comparative example is the same as that of Example 1

[0082] Table 9 Recipe

[0083] Component A Dosage wt% Dicyclopentadiene resin 60 Styrene 10 Dispersant BYK190 4 Defoamer TEGO825 1.9 Wetting agent TEGO254 0.8 Rust inhibitor CK34 0.7 Leveling agent BYK307 1.3 Zinc phosphate anti-rust pigment 14.6 Aniline Black 4.9 Silicone surfactant MY1291 1.5 Gemini surfactant Surfynol104E 0.3

[0084] The component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.3:1.2.

[0085] The mass ratio of component A to component B is 100:2.5.

[0086] The Gemini surfactant Surfyno l 104E was purchased from Evonik in the United States and is a Gemini nonionic surfactant.

[0087] Performance Testing

[0088] Performance test 1: impact resistance (GB / T1732-2020);

[0089] Performance test 2: Coloring ability test, refer to "Research on the preparation technology of high-quality nano iron oxide red paint for automobiles", Modern coatings and coatings, Guo Xiaoyao et al.; 1.2.1 Color tinting strength evaluation index;

[0090] Performance test 3: Storage stability (GB / T6753.3-1986);

[0091] Performance test 4: paint film adhesion (GB / T9286-1998);

[0092] Performance test 5: paint film hardness (GB / T1730-1993);

[0093] Performance test 6: gloss (GB / T1743-1989);

[0094] Performance Test 7: Curing time at 25°C and 50% relative humidity (min);

[0095] Performance Test 8: Sandability: Use 500-grit sandpaper to sand the car paint that has been shade-dried for 24 hours. Visually observe the amount of powder produced after sanding for 30 seconds. The grades are divided into extremely easy to sand, easy to sand, sandable, and difficult to sand.

[0096] The performance test results can be found in Table 10;

[0097] Table 10 Test results

[0098]

[0099] The putty for light alloy provided by the present invention is based on dicyclopentadiene resin as main film-forming material, and curing agent selects to use benzoyl peroxide (BPO), peroxy neodecanoate tert-butyl ester, and two substances are mixed and used to improve the curing efficiency of dicyclopentadiene resin. In addition, the application uses organosilicon surfactant, carboxylate type gemini surfactant and aniline black, and organosilicon surfactant MY1291 is a kind of water-based system organosilicon surfactant, which can reduce surface tension so that coating has good wettability and leveling, and gemini surfactant CGS-2 can make the paint surface tighter, and has certain metal anticorrosion effect, but the effect of the two used alone is not ideal, and it is shared with aniline black compared to carbon black with certain tinting strength and glossiness, and lacks organosilicon surfactant MY1291, and tinting strength is reduced, and after lacking gemini surfactant CGS-2, tinting strength is reduced, and storage performance decreases.

[0100] It can be seen that the two surfactants are indispensable, and the colorant should be used together with the two surfactants to achieve the best gloss, tinting strength, and anti-corrosion performance. If the Gemini nonionic surfactant is used instead, the tinting strength %, storage stability, and gloss are not as good as the carboxylate Gemini surfactant CGS-2. In addition, the carboxylate Gemini surfactant CGS-2, the silicone surfactant MY1291, and aniline black are indispensable, and have a significant impact on gloss, tinting strength, and anti-corrosion performance.

[0101] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A putty for light alloy, characterized in that: The invention is composed of component A and component B, wherein component A comprises the following components in parts by mass: 5-20 parts of styrene, 45-60 parts of dicyclopentadiene resin, 0.5-5 parts of dispersant, 0.1-1 parts of defoamer, 0.1-1 parts of wetting agent, 0.1-1 parts of rust inhibitor, 15-20 parts of zinc phosphate rust-proof pigment, 1-7 parts of aniline black, 1-2 parts of leveling agent, 1-1.5 parts of organosilicon surfactant, and 0.1-0.5 parts of carboxylate type gemini surfactant; component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of (0.7-1.5): (0.8-1.5); the mass ratio of component A to component B is 100: (1.5-3); the product specification of the organosilicon surfactant is MY1291, which is purchased from Anhui Mingyi Co., Ltd.; the carboxylate type gemini surfactant is a carboxylate type gemini surfactant The agent CGS-2 is prepared by the following process: 10g N, N'-didodecylethylenediamine and 7.6g succinic anhydride are dissolved in 50mL tetrahydrofuran, and the mixture is reacted at 70°C for 24h. After the reaction is completed, the solvent is evaporated under reduced pressure to obtain a white powder solid A. The obtained solid A is dispersed in 100mL deionized water, the pH is adjusted to 10 with a NaOH solution, the insoluble matter is filtered out, the filtrate is collected, the pH of the filtrate is adjusted to 2 with hydrochloric acid, the insoluble matter is collected, and the solid B is washed with distilled water until neutral to obtain a solid B, which is then recrystallized twice with a mixed solvent of ethyl acetate and ethanol, wherein the volume ratio of ethyl acetate to ethanol is 1:3, to obtain a white powder solid C. The obtained solid C is dissolved in an ethanol solution of NaOH, the solvent is evaporated under reduced pressure, and the obtained solid D is dispersed in chloroform, the insoluble matter is filtered out, and the solvent is evaporated to obtain the carboxylate type gemini surfactant CGS-2.

2. The putty for light alloy according to claim 1, wherein: The component A comprises the following components in parts by mass: 12.5 parts of styrene, 57 parts of dicyclopentadiene resin, 4 parts of dispersant, 1 part of defoamer, 0.5 parts of wetting agent, 0.5 parts of rust inhibitor, 16.5 parts of zinc phosphate rust-proof pigment, 5 parts of aniline black, 1.5 parts of leveling agent, 1 part of silicone surfactant, and 0.5 parts of carboxylate gemini surfactant; the component B is prepared by mixing benzoyl peroxide and tert-butyl peroxyneodecanoate in a mass ratio of 1.5:1; the mass ratio of component A to component B is 100:2.

5.

3. The putty for lightweight alloy as claimed in claim 2, wherein the dispersant is a German BYK brand, model BYK190; the defoamer is a German Digo brand, model TEGO825; the rust inhibitor is Qingdao Enze, model anti-flash rust agent CK34; the leveling agent is a German BYK, model BYK307.

4. The putty for lightweight alloy as claimed in claim 1, wherein the zinc phosphate antirust pigment is purchased from Jinan Quanxing New Materials Co., Ltd.

5. The method for preparing a putty for a light alloy as claimed in claim 4, comprising the following steps: S1. First, component A is prepared according to the mass ratio, styrene, dicyclopentadiene resin, silicone surfactant MY1291, carboxylate type gemini surfactant CGS-2, and dispersant BYK190 are first mixed evenly, zinc phosphate antirust pigment and aniline black are added in a dispersed state, and after mixing evenly, the remaining components of component A are added, dispersed and stirred evenly to obtain a uniformly mixed component A, and then component B is prepared according to the mass ratio, benzoyl peroxide and tert-butyl peroxyneodecanoate are added, and stirred evenly to obtain a uniformly mixed component B; S2. Before use, mix the uniformly mixed component A and the uniformly mixed component B in the mass ratio.

6. The method for using the putty for light alloy as claimed in claim 4, comprising the following steps: S1. Remove oil, rust, old paint film and moisture from the surface of the coating before use, and keep the surface clean and dry; S2. Blend component A and component B in a mass ratio of 100:(1.5-3) to obtain a putty with uniform color; S3. Apply the putty obtained in S2 within 15 minutes.

7. The method for using the putty for light alloy as claimed in claim 6, further comprising step S4 after step S3, wherein after the application is completed, dry grinding is performed after the putty is completely hardened.

8. The method for using the putty for light alloy as claimed in claim 7, wherein the coating surface in step S1 refers to one or more of a glass fiber reinforced plastic surface, an iron plate surface, a steel plate surface, an aluminum plate surface, and a galvanized plate surface.

Citation Information

Cited By

  • Light energy metal plate putty as well as preparation method and application thereof

    CN121873597A

  • A light energy metal plate putty, a preparation method and application thereof

    CN121873597B