A Yolk-shell alloy catalyst, synthesis method and application thereof

Through the synthesis of Yolk-shell type Pd-M@mSiO2 alloy catalyst, the problems of poor stability and inconsistent catalytic effect of existing catalysts are solved, and efficient catalytic hydrogenation of levulinic acid to prepare γ-valerolactone is achieved with good catalytic activity. and reusability.

CN118304883BActive Publication Date: 2024-10-25QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410402310.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-10-25
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

Existing catalysts have poor stability and poor reusability when catalyzing the hydrogenation of levulinic acid to produce γ-valerolactone, and the Yolk-shell core-shell catalyst has inconsistent catalytic effects in different hydrogenation reactions.

Method used

The synthesis method of Yolk-shell type Pd-M@mSiO2 alloy catalyst is used to form PdO-MxOy@mSiO2 with a uniform pore structure through the reaction of CTAB, K2PdCl4, metal M salt and NaOH, and then reduced in a hydrogen atmosphere. A Pd-M@mSiO2 alloy core-shell catalyst was obtained, which was used to catalyze the hydrogenation of levulinic acid to prepare γ-valerolactone.

Benefits of technology

The catalytic activity and selectivity are improved, the reaction by-products are less, the catalyst can be directly recycled for more than 10 times, the catalytic performance is stable, the morphology is regular, and the appropriate active sites promote the reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118304883B_ABST
    Figure CN118304883B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of catalytic technology, and relates to a Yolk-shell alloy catalyst, a synthesis method and its application. The Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention has high catalytic activity and selectivity when catalyzing the hydrogenation of levulinic acid to prepare γ-valerolactone; the obtained by-products are few, and the product post-processing is simple; after the hydrogenation reaction of levulinic acid is completed, the catalyst and the product can be separated simply and efficiently by centrifugation, and the catalyst phase does not need post-processing, and can be directly reused. After being reused 10 times, the catalytic performance is not significantly reduced, and the recycling effect is good. The preparation method of the alloy catalyst Pd-M@mSiO2 provided by the present invention is simple, and the synthesized Yolk-shell alloy catalyst has a regular morphology, and has high catalyst stability, catalytic activity and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysis, and relates to a Yolk-shell alloy catalyst, a synthesis method and applications thereof, and specifically relates to a Yolk-shell alloy catalyst and a synthesis method thereof, and a method for preparing gamma-valerolactone by catalyzing hydrogenation of levulinic acid using the Yolk-shell alloy catalyst. Background Art

[0002] Due to the adverse effects of traditional fuels and fuel additives from fossil fuels, the modern world prioritizes the volatilization of biomass into value-added chemicals, fuels, and fuel additives. Under the global theme of advocating carbon neutrality and low-carbon economy, the value-added of biomass resources has aroused great interest among researchers around the world. It can not only develop effective technologies, but also solve the utilization of agricultural and forestry wastes at the same time, and the utilization of bioproducts is becoming crucial. Among them, levulinic acid (LA) is considered to be an important bio-based platform chemical and is praised by the United States as one of the "twelve major platform molecules" derived from biomass. Selective hydrogenation of LA or its esters can produce a variety of high-value-added derivatives, including γ-valerolactone (GVL), 1,4-pentanediol (PDO), 2-methyl-tetrahydrofuran (MTHF) and valeric acid. Among these biomass-derived compounds, GVL is widely used, not only as a food ingredient, green solvent, and pharmaceutical intermediate, but also as an advanced renewable fuel and other commercial uses.

[0003] At present, the catalysts commonly used to catalyze the hydrogenation of levulinic acid to prepare γ-valerolactone mainly include noble metal (Ru, Pt, Pd, Au) and non-noble metal (Ni, Cu, Co) based catalysts. Chinese patent CN111036239B discloses the preparation of γ-valerolactone from levulinic acid using a supported sulfide catalyst, wherein the active metal is supported on a catalyst carrier, and the catalyst carrier is selected from carbon, ZrO2 or Al2O3; in addition, Chinese patent CN113441143B adopts a nickel-cobalt-aluminum ternary metal composite catalyst to catalyze the hydrogenation of levulinic acid to prepare γ-valerolactone. The above catalysts are all supported catalysts. Although the production of γ-valerolactone is promoted to a certain extent, the stability of the catalyst itself is poor, and the active metal is easy to sinter and leach, resulting in poor reusability of the catalyst.

[0004] In recent years, Yolk-shell core-shell catalysts have attracted widespread attention from researchers. Yolk-shell core-shell catalysts are nanoreactors that encapsulate particles in a hollow shell. Compared with commonly used core-shell core-shell catalysts, they have a movable active core, a large cavity structure and a porous shell, and have the advantages of controlling the reaction microenvironment, confinement effect, and dividing or accumulating various types of basic reactions. Compared with supported catalysts, the cavity part of the Yolk-shell core-shell catalyst can enrich more reactants to participate in the catalytic reaction, which is beneficial to increase the reaction rate. At the same time, the shell acts as a protective layer to prevent the agglomeration of the core. Among them, Pd-based core-shell catalysts not only have excellent hydrogenation activity, but also have excellent hydrogenation / hydrogenolysis selectivity for C=O / CO bonds, and are widely used in hydrogenation reactions. In addition, the catalytic performance of the catalyst can be improved by further modification such as the introduction of other active metals. However, in different hydrogenation reactions, the shells and cores of different components and modification methods have different catalytic effects. The selection of appropriate modification methods has a great promoting effect on improving the yield of the target product. Among them, alloys are widely studied due to their excellent hydrogenation ability. Therefore, it has become an urgent problem to study and develop a Pd-based Yolk-shell alloy catalyst that has good catalytic performance in catalyzing the hydrogenation of levulinic acid to prepare γ-valerolactone. Summary of the invention

[0005] In view of this, the present invention provides a Yolk-shell alloy catalyst, a synthesis method and an application thereof. The Yolk-shell alloy catalyst can effectively catalyze the hydrogenation of levulinic acid to prepare γ-valerolactone.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The first object of the present invention is to provide a method for synthesizing a Yolk-shell type alloy catalyst, the method comprising the following steps:

[0008] S1, mixing hexadecyltrimethylammonium bromide (CTAB) with deionized water, adding K2PdCl4 salt and salt solution of metal M after stirring and heating, continuing to stir, adding ascorbic acid aqueous solution dropwise, stirring to obtain a colloidal solution of metal Pd and M;

[0009] S2, adding a certain concentration of NaOH solution to the colloidal solution of metal Pd and metal M, adjusting the pH value of the solution, then dropping tetraethyl orthosilicate (TEOS) solution to initiate silica gel polymerization reaction, then dropping 1,2-bis(trimethoxysilyl)ethane (BTME) solution to react, centrifuging to obtain the product Pd-M@SiO2, and then drying at a certain temperature;

[0010] S3, calcining the dried Pd-M@SiO2 to obtain PdO-M with uniform pore structure x O y @mSiO2;

[0011] S4, PdO-M with uniform pore structure x O y @mSiO2 was reduced in a hydrogen atmosphere to obtain Yolk-shell type Pd@mSiO2-M x O y Alloy core-shell catalyst.

[0012] Furthermore, the above synthesis method has the following more specific steps:

[0013] S1. Mix 0.10-0.15g CTAB with 45mL deionized water in a flask, raise the temperature to 95°C and maintain for 30min, then add 5-10mL 0.02mol / L K2PdCl4 and metal M salt solution respectively, continue stirring for 10-30min, the solution changes from colorless and transparent to orange-red, add ascorbic acid aqueous solution, continue stirring for 30-60min, and obtain a colloidal solution of metal Pd and metal M;

[0014] S2. Add 2-5 mL of 0.5 mol / L NaOH solution to the colloidal solution, adjust the pH value of the solution to 10-11, then add 0.4-0.45 mL of TEOS solution to initiate silica gel polymerization reaction, stir for 1-3 h, add 0.3-0.4 mL of BTME solution to react for 40-80 min, centrifuge to obtain Pd-M@SiO2 product, and dry at 60-80 °C for 8-10 h;

[0015] S3, the dried Pd-M@SiO2 was calcined in a muffle furnace, the temperature was raised to 450-500°C at a rate of 1-3°C / min, and the calcination time was 3-5h, to obtain a Yolk-shell catalyst PdO-M with a cavity and uniform pore structure. x O y @mSiO2.

[0016] S4, the obtained PdO-M x O y The @mSiO2 catalyst was reduced at a flow rate of 40-60 mL / min of H2 and a temperature of 200-500°C for 4-6 h to finally obtain a Yolk-shell type Pd-M@mSiO2 alloy core-shell catalyst.

[0017] It should be noted that the preparation steps of the Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention are simple. The Yolk-shell alloy catalyst Pd-M@mSiO2 has an alloy core of metal as a hydrogenation active site and a shell of SiO2 with uniform pores, so that the obtained nano alloy material Pd-M@mSiO2 can catalyze the hydrogenation of levulinic acid to prepare γ-valerolactone.

[0018] If the Yolk-shell catalyst has an irregular morphology, it will cause the reactant molecules to be blocked. The modification method provided by the present invention will not destroy the original core-shell morphology of the catalyst Pd-M@mSiO2, which is conducive to the reactant molecules passing through the shell to contact the active metal inside; and in the reaction of catalyzing the hydrogenation of levulinic acid to prepare γ-valerolactone, the appropriate type and number of active sites are the key to catalytic performance. The modification method provided by the present invention can obtain the Pd-M alloy without destroying the original Yolk-shell core-shell structure, thereby promoting the reaction.

[0019] Preferably, the M metal salt is selected from one of Ce(NO3)3·6H2O, Al(NO3)3·9H2O, Zr(NO3)4·5H2O, Ni(NO3)2·6H2O, Co(NO3)2·6H2O, Mg(NO3)2·6H2O, Fe(NO3)3·9H2O, Cu(NO3)2·6H2O, Zn(NO3)2·6H2O, and Mn(NO3)2·4H2O.

[0020] The synthesis mechanism of the modified Yolk-shell alloy catalyst Pd-M@mSiO2 described in the present invention is as follows Figure 1 shown.

[0021] The second object of the present invention is to provide a Yolk-shell alloy catalyst Pd-M@mSiO2 prepared according to the above synthesis method.

[0022] The third invention objective of the present invention is to provide a method for preparing γ-valerolactone by hydrogenating levulinic acid catalyzed by the alloy core-shell catalyst Pd-M@mSiO2. The Yolk-shell alloy catalyst Pd-M@mSiO2 catalyzes the hydrogenation of levulinic acid to prepare γ-valerolactone.

[0023] Preferably, the catalytic hydrogenation reaction is carried out in a stainless steel high-pressure reactor. The air in the reactor is first replaced with nitrogen several times and then pressurized hydrogen is filled in. The hydrogenation reaction is carried out by heating and stirring.

[0024] Furthermore, the mass ratio of the Yolk-shell alloy catalyst Pd-M@mSiO2 to levulinic acid is 1:3-15, the reaction temperature is 140-180°C, the hydrogen pressure is 1.0-3.0MPa, and the reaction time is 3.0-5.0h.

[0025] After the catalytic hydrogenation reaction of the catalyst provided by the present invention is completed, the catalyst Pd-M@mSiO2 and the product γ-valerolactone are recovered by centrifugation, and the catalyst phase does not need to be post-treated and is directly recycled.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) The Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention has high catalytic activity and selectivity when catalyzing the hydrogenation of levulinic acid to prepare γ-valerolactone; less by-products are obtained after the reaction, and the post-treatment of the product is simple; after the hydrogenation reaction of levulinic acid is completed, the catalyst and the product can be separated simply and efficiently by centrifugation, and the catalyst phase does not need post-treatment and can be directly reused. After being reused 10 times, the catalytic performance is not significantly reduced, and the recycling effect is good.

[0028] 2) The preparation method of the alloy catalyst Pd-M@mSiO2 provided by the present invention is simple. The Yolk-shell alloy catalyst synthesized by the method provided by the present invention has a regular morphology. The catalyst catalyzes the hydrogenation of levulinic acid to prepare γ-valerolactone and has high catalyst stability, catalytic activity and reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0030] Figure 1 Schematic diagram of the synthesis of the Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention.

[0031] Figure 2 TEM images of the Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention; (a) Pd-Ce@mSiO2, (b) Pd-Al@mSiO2, (c) Pd-Co@mSiO2. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.

[0034] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.

[0035] Example 1 Synthesis of Yolk-shell alloy catalyst Pd-Ce@mSiO2

[0036] S1. Mix 0.10 g CTAB with 45 mL deionized water in a flask, raise the temperature to 95 °C, stir continuously and maintain for 30 min, then add 5 mL 0.02 mol / L K2PdCl4 and Ce(NO3)3·6H2O salt solution, continue stirring for 15 min, the solution changes from colorless and transparent to orange-red, add ascorbic acid aqueous solution, continue stirring for 30 min, and obtain a colloidal solution of metal Pd and Ce;

[0037] S2, add 2.5mL 0.5mol / LNaOH solution to the above colloidal solution, adjust the solution pH to about 10-11, then drop 0.42mL TEOS solution to initiate silica gel polymerization reaction, add 0.3mL BTME solution after 3h to react for 50min, centrifuge to obtain Pd-Ce@SiO2 product, and dry at 60°C;

[0038] S3, calcining the dried Pd-Ce@SiO2 in a muffle furnace, wherein the temperature is increased from 2°C / min to 500°C for 3 hours to obtain powdered PdO-CeO2@mSiO2;

[0039] S4. Reduce the obtained powder PdO-CeO2@mSiO2 under H2 at a flow rate of 60 mL / min and a temperature of 500°C for 4 h to finally obtain a Yolk-shell type alloy catalyst PdO-CeO2@mSiO2.

[0040] Example 2 Synthesis of Yolk-shell alloy catalyst Pd-Al@mSiO2

[0041] S1. Mix 0.12 g CTAB with 50 mL deionized water in a flask, raise the temperature to 95 °C, keep stirring and maintain for 30 min, then add 7 mL 0.02 mol / L K2PdCl4 and Al(NO3)3·9H2O salt solution respectively, continue stirring for 15 min, the solution changes from colorless and transparent to orange-red, add ascorbic acid aqueous solution dropwise, continue stirring for 40 min, and obtain a colloidal solution of metal Pd and Al;

[0042] S2, add 2.2mL 0.5mol / LNaOH solution to the above colloidal solution, adjust the solution pH to about 10-11, then drop 0.40mL TEOS solution to initiate silica gel polymerization reaction, add 0.36mL BTME solution after 3h to react for 60min, centrifuge to obtain Pd-Al@SiO2 product, and dry at 80℃;

[0043] S3, calcining the dried Pd-Al@SiO2 in a muffle furnace, the temperature during calcination is increased from 2°C / min to 450°C, the calcination time is 3h, and powder PdO-Al2O3@mSiO2 is obtained;

[0044] S4. The obtained powder PdO-Al2O3@mSiO2 was reduced at 500°C for 5 h at a flow rate of 60 mL / min of H2 to finally obtain a Yolk-shell type alloy catalyst Pd-Al@mSiO2.

[0045] Example 3 Synthesis of Yolk-shell Type Catalyst Pd-Co@mSiO2

[0046] S1. Mix 0.11 g CTAB with 45 mL deionized water in a flask, raise the temperature to 95 °C, keep stirring and maintain for 30 min, then add 8 mL 0.02 mol / L K2PdCl4 and Co(NO3)2·6H2O salt solution respectively, continue stirring for 10 min, the solution changes from colorless and transparent to orange-red, add ascorbic acid aqueous solution, continue stirring for 45 min, and obtain a colloidal solution of metal Pd and Co;

[0047] S2, add 2.7mL 0.5mol / LNaOH solution to the above colloidal solution, adjust the solution pH to about 10-11, then drop 0.44mL TEOS solution to initiate silica gel polymerization reaction, add 0.4mL BTME solution after 2h to react for 70min, centrifuge to obtain Pd-Co@SiO2 product, and dry at 80°C;

[0048] S3, calcining the dried Pd-Co@SiO2 in a muffle furnace, the temperature during calcination is increased from 2°C / min to 550°C, the calcination time is 3h, and powder PdO-Co2O3@mSiO2 is obtained;

[0049] S4. The obtained powder PdO-Co2O3@mSiO2 was reduced at 500°C for 4 h at a flow rate of 60 mL / min of H2 to finally obtain a Yolk-shell type alloy catalyst Pd-Co@mSiO2.

[0050] Example 4 Synthesis of Yolk-shell Type Catalyst Pd-Ni@mSiO2

[0051] S1. Mix 0.15g CTAB with 60mL deionized water in a flask, raise the temperature to 95°C, stir continuously and maintain for 30min, then add 5.5mL 0.02mol / L K2PdCl4 and Ni(NO3)2·6H2O salt solution respectively, continue stirring for 15min, the solution changes from colorless and transparent to orange-red, add ascorbic acid aqueous solution, continue stirring for 60min, and obtain a colloidal solution of metal Pd and Ni;

[0052] S2. Add 2 mL of 0.5 mol / L NaOH solution to the colloidal solution to adjust the pH value of the solution to about 10-11, then drop 0.45 mL of TEOS solution to initiate silica gel polymerization reaction, add 0.32 mL of BTME solution after 3 hours to react for 50 minutes, centrifuge to obtain Pd-Ni@SiO2 product, and dry at 60°C;

[0053] S3, calcining the dried Pd-Ni@SiO2 in a muffle furnace, the temperature during calcination is increased from 1°C / min to 550°C, the calcination time is 4h, to obtain powder PdO-NiO@mSiO2;

[0054] S4. The obtained powder PdO-NiO@mSiO2 was reduced at a flow rate of 60 mL / min of H2 and a temperature of 500°C for 6 h to finally obtain a Yolk-shell type alloy catalyst Pd-Ni@mSiO2.

[0055] Furthermore, if Figure 2TEM images of the Yolk-shell alloy catalyst Pd-M@mSiO2 provided by the present invention; (a) Pd-Ce@mSiO2, (b) Pd-Al@mSiO2, (c) Pd-Co@mSiO2. As can be seen from the figure, all the alloy catalysts have a clear and regular core-shell structure with uniform particle size, the metal alloy cores are randomly distributed in the cavity size, and the catalyst worm-like channels and large cavity size are more obvious. The above characteristics indicate that the Yolk-shell alloy catalyst Pd-M@mSiO2 was successfully synthesized.

[0056] Example 5 Method for preparing γ-valerolactone by hydrogenation of levulinic acid catalyzed by Pd-Ce@mSiO2

[0057] 1.0g of levulinic acid and 0.2g of Pd-Ce@mSiO2 prepared in Example 1 were added to a stainless steel autoclave, and the air in the autoclave was replaced with nitrogen 5 times, followed by 3.0MPa of hydrogen. The autoclave was heated and stirred at 160°C for 5h, and then cooled to room temperature. Under the action of high-speed centrifugation, the product phase was separated from the catalyst phase, and the separated catalyst could be directly recycled without post-treatment. The conversion rate of levulinic acid was 100%, the selectivity of γ-valerolactone was 97%, and the calculation formulas of the conversion rate of levulinic acid and the yield of γ-valerolactone were as follows:

[0058]

[0059]

[0060] Example 6 Method for preparing γ-valerolactone using levulinic acid catalyzed by Pd-Al@mSiO2

[0061] 1.0 g of levulinic acid and 0.25 g of Pd-Al@mSiO2 synthesized in Example 2 were added to a stainless steel autoclave, and the air in the autoclave was replaced with nitrogen 5 times, and then filled with 2.0 MPa of hydrogen. The autoclave was heated and stirred at 150°C for 4 h, and then allowed to stand and cool to room temperature. Under the action of high-speed centrifugation, the product phase was separated from the catalyst phase, and the separated catalyst could be directly recycled without post-treatment. The conversion rate of levulinic acid was 99.5%, and the selectivity of γ-valerolactone was 99%.

[0062] Example 7 Method for preparing γ-valerolactone using levulinic acid catalyzed by Pd-Co@mSiO2

[0063] 1.5 g of levulinic acid and 0.3 g of Pd-Co@mSiO2 synthesized in Example 3 were added to a stainless steel autoclave, and the air in the autoclave was replaced with nitrogen 4 times, and then filled with 3.0 MPa of hydrogen. The autoclave was heated and stirred at 180°C for 3 h, and then allowed to stand and cool to room temperature. Under the action of high-speed centrifugation, the product phase was separated from the catalyst phase, and the separated catalyst could be directly recycled without post-treatment. The conversion rate of levulinic acid was 98.9%, and the selectivity of γ-valerolactone was 99.6%.

[0064] Example 8 Method for preparing γ-valerolactone using levulinic acid catalyzed by Pd-Ni@mSiO2

[0065] 1.2 g of levulinic acid and 0.15 g of Pd-Ni@mSiO2 synthesized in Example 1 were added to a stainless steel autoclave, and the air in the autoclave was replaced with nitrogen for 6 times, and then filled with 3.0 MPa of hydrogen. The autoclave was heated and stirred at 170°C for 5 h, and then allowed to stand and cool to room temperature. Under the action of high-speed centrifugation, the product phase was separated from the catalyst phase, and the separated catalyst could be directly recycled without post-treatment. The conversion rate of levulinic acid was 100%, and the selectivity of γ-valerolactone was 98.1%.

[0066] Example 9 Catalytic performance test of the catalyst after repeated use

[0067] The experimental conditions and steps were the same as those in Example 1, except that the catalyst was replaced with the catalyst recovered in Example 1. The experiment was repeated 10 times. After repeated use 10 times, the conversion rate of levulinic acid was 99.3%, and the selectivity of γ-valerolactone was 96.8%.

[0068] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a Yolk-shell alloy catalyst Pd-M@mSiO2, characterized in that: The following steps are involved: S1. Mix cetyltrimethylammonium bromide (CTAB) with water, add K2PdCl4 and a salt solution of metal M after stirring and heating, continue stirring, dropwise add an aqueous solution of ascorbic acid, and stir to obtain a colloidal solution of the corresponding metal; M metal salt is selected from one of Ce(NO3)3·6H2O and Al(NO3)3·9H2O; S2, adding NaOH solution to the colloidal solution to adjust the pH value of the solution, then dropping TEOS solution to initiate silica gel polymerization reaction, and finally dropping BTME solution to react, and centrifuging to obtain the product Pd-M@SiO2; S3, calcining the product Pd-M@SiO2 to obtain a PdO-MxOy@mSiO2 catalyst with uniform pores; S4, reducing the PdO-MxOy@mSiO2 catalyst under the action of hydrogen to obtain a Yolk-shell alloy catalyst Pd-M@mSiO2; The alloy catalyst Pd-M@mSiO2 has a clear and regular core-shell structure with uniform particle size, the metal alloy cores are randomly distributed in the cavity size, and the catalyst worm-like pores and large cavity size are more obvious.

2. The method for preparing Yolk-shell type alloy catalyst Pd-M@mSiO2 according to claim 1, characterized in that: The specific steps include: S1. Mix 0.10-0.15 g CTAB and 45-60 mL deionized water in a flask, heat to 95° C. and stir continuously for 30 min, then add 5-10 mL 0.02 mol / L Pd and metal M salt solutions respectively, continue stirring for 10-30 min, add ascorbic acid aqueous solution, continue stirring for 30-60 min, and obtain a colloidal solution of precious metal Pd and metal M; S2. Add 2-5 mL of 0.5 mol / L NaOH solution to the obtained colloidal solution, adjust the pH value of the solution to 10-11, then drop 0.40-0.45 mL of TEOS solution to initiate silica gel polymerization reaction, stir for 1-3 h, then drop 0.3-0.4 mL of BTME solution to react for 40-80 min, centrifuge to obtain Pd-M@SiO2 product, and dry at 60-80 ° C for 8-10 h; S3, calcining the product Pd-M@SiO2 after drying overnight in a muffle furnace, and the temperature during calcination is increased to 450-550°C at a rate of 1-3°C / min, and the calcination time is 3-5h to obtain a catalyst PdO-MxOy@mSiO2 with a pore structure; S4. Reduce the obtained catalyst PdO-MxOy@mSiO2 at a flow rate of 40-60 mL / min of H2 and a temperature of 200-500°C for 4-6 hours to finally obtain a Yolk-shell type alloy catalyst Pd-M@mSiO2.

3. A Yolk-shell alloy catalyst Pd-M@mSiO2 prepared by the method as described in any one of claims 1-2.

4. Use of a Yolk-shell alloy catalyst Pd-M@mSiO2 prepared by the method according to any one of claims 1 to 2 in the field of catalysis.

5. The use according to claim 4, characterized in that: The Yolk-shell alloy catalyst Pd-M@mSiO2 catalyzes the hydrogenation of levulinic acid to prepare γ-valerolactone.

6. The use according to claim 5, characterized in that: The catalytic hydrogenation reaction is carried out in a stainless steel high-pressure reactor. The air in the reactor is first replaced with nitrogen several times and then pressurized hydrogen is filled in. The hydrogenation reaction is carried out by heating and stirring.

7. The use according to claim 5 or 6, characterized in that: The mass ratio of the Yolk-shell alloy catalyst Pd-M@mSiO2 to levulinic acid is 1:3-15, the reaction temperature is 140-180°C, the hydrogen pressure is 1.0-3.0MPa, and the reaction time is 3.0-5.0h.

8. The use according to claim 5 or 6, characterized in that: After the catalytic hydrogenation reaction is completed, the catalyst Pd-M@mSiO2 and the product γ-valerolactone are recovered by centrifugation, and the catalyst phase can be directly recycled without post-treatment.