A method for preparing highly corrosion-resistant and wear-resistant composite floor

By coating the surface of the wear-resistant layer of the composite floor with a corrosion-resistant coating made of nanomaterials, combined with fillers such as zirconia ceramics and silicon carbide, the problem of insufficient wear resistance and corrosion resistance of the composite floor is solved, achieving a higher Wear and corrosion resistance extend service life.

CN118306096BActive Publication Date: 2024-10-08SHANGHAI JUYUAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410574543.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-08
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

Existing composite floors have limited wear resistance and corrosion resistance, making it difficult to meet high-demand usage environments.

Method used

A composite floor consisting of a wear-resistant layer, a decorative layer, and a base material layer is used. By coating the surface of the wear-resistant layer with a corrosion-resistant coating, nano-titanium dioxide, mica iron oxide, polydopamine and other materials are used to prepare the corrosion-resistant coating, combined with oxidation Fillers such as zirconium ceramics and silicon carbide improve the wear resistance and corrosion resistance of the floor.

Benefits of technology

It significantly improves the wear resistance and corrosion resistance of composite flooring, can resist the erosion of environmental factors, prolongs the service life, and enhances the adhesion and durability of the coating through polydopamine modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004832005790000111
    Figure BDA0004832005790000111
  • Figure BDA0004832005790000121
    Figure BDA0004832005790000121
Patent Text Reader

Abstract

The present invention relates to a method for preparing a highly corrosion-resistant and wear-resistant composite floor, and belongs to the technical field of composite floor. The composite floor material of the present invention is prepared from a wear-resistant layer, a decorative layer, a substrate layer, and a balancing layer from top to bottom by hot pressing, heat preservation and pressure preservation, and a corrosion-resistant coating is added to the surface of the wear-resistant layer by electrostatic spraying, so that the floor has better corrosion resistance. Compared with the prior art, the composite floor prepared by the present invention not only improves the wear resistance of the wear-resistant layer, but also has excellent corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite floors and relates to a method for preparing a highly corrosion-resistant and wear-resistant composite floor. Background Art

[0002] Compared with traditional floors such as solid wood floors and tile floors, laminate floors have the following advantages: more affordable. Compared with solid wood floors, laminate floors use more diverse raw materials and are more affordable. Laminate floors are more adaptable, not only to floor heating, but also to environments with high humidity, and are not easy to deform or crack. In addition, laminate floors are simple and convenient to install, do not require putty, and have a short installation cycle, which greatly reduces the difficulty and pollution of construction. The surface of the laminate floor uses a high-quality wear-resistant coating, which has good waterproof, moisture-proof, anti-fouling and anti-scratch properties. Usually, you only need to use a mop and detergent for simple cleaning and maintenance.

[0003] Composite flooring is a flooring made of multiple layers of materials. In the prior art, high-strength and high-wear-resistant surface materials such as high-density fiberboard, epoxy resin, aluminum oxide, etc. are usually used to improve the wear resistance of composite flooring. At the same time, surface coating is used to enhance the wear resistance of composite flooring, and the floor is textured to increase the friction of the floor surface, improve the anti-slip and wear resistance of the floor. Common treatment methods include notching, embossing, and concave-convex. In the prior art, corrosion resistance is usually achieved by improving the surface coating. Common surface coatings include UV coating, frosted paint coating, metal oxide coating, etc.

[0004] However, the above technologies have limited effect on improving the wear resistance and corrosion resistance of the composite floor, so it is necessary to develop a composite floor with excellent corrosion resistance and wear resistance. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a highly corrosion-resistant and wear-resistant composite floor, which has better wear resistance and corrosion resistance.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a highly corrosion-resistant and wear-resistant composite floor, the wooden floor is composed of a wear-resistant layer, a decorative layer, a substrate layer, and a balancing layer from top to bottom, wherein a corrosion-resistant coating is coated on the surface of the wear-resistant layer. The specific preparation process of the composite floor is as follows:

[0008] S1. In parts by weight, 10 parts of polyvinyl alcohol, 1 to 2 parts of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics are mixed by ultrasonic mixing for 2 to 3 hours, and the mixture is heated to 60 to 80° C. and dried by hot air to obtain modified zirconia ceramics;

[0009] 2-4 parts of stearic acid, 60-75 parts of aluminum oxide, 10-15 parts of modified zirconia ceramics, 10-25 parts of silicon carbide, and 5-10 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 hours, and fully mixed to obtain a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 3-4 hours at 40-50° C., and after mixing, the solution was filtered to obtain a modified filler.

[0010] S2, dispersing 10 to 20 parts of the modified filler into 50 to 60 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer;

[0011] S3, ultrasonically dispersing 5 to 8 parts of nano titanium dioxide and 3 to 5 parts of mica iron oxide in 70 to 100 parts of deionized water, adding 1.5 parts of dopamine hydrochloride solution, and maintaining the solution pH at 8.0 to 9.0; stirring the reaction in a magnetic stirrer for 1 to 2 hours, then adding 0.5 to 1 part of silane coupling agent, and continuing to stir the reaction at 70 to 80° C. for 3 hours to obtain a polydopamine-modified nanofiller;

[0012] Put it into a ball mill and grind it at a speed of 300r / min for 4h, sieve it through 200 mesh to obtain nano filler powder, add 10-15 parts of nano filler powder, 40-50 parts of polyvinyl alcohol, 20-30 parts of polyvinylidene fluoride resin, 2-5 parts of curcumin and 2-5 parts of dispersant into the reactor, mix and stir, stir at a speed of 800-1000r / min for 1-2h, and the reaction temperature is 70-80°C to obtain a corrosion-resistant coating;

[0013] S4, grinding the surface of the wear-resistant layer to a thickness of 0.1 to 0.3 mm, and spraying a corrosion-resistant coating on the ground surface of the wear-resistant layer by electrostatic spraying;

[0014] S5, heating and curing the coating obtained in S4 at 160-180° C. for 1-2 hours to obtain the corrosion-resistant coating;

[0015] S6. Purging and drying each layer of the structure with nitrogen at 70°C;

[0016] S7. Assemble the composite floor in the order of balancing layer, adhesive, base material layer, adhesive, decorative layer, adhesive and wear-resistant layer from bottom to top by hot pressing at a temperature of 160-180°C and a pressure of 0.2-0.5 MPa for 10-20 minutes using a hot press, and then keep the heat and pressure at a temperature of 130-150°C and a pressure of 0.1-0.4 MPa for 10 hours to obtain the highly corrosion-resistant and wear-resistant composite floor.

[0017] As a preferred technical solution of the present invention, the substrate layer is a double-layer solid wood board, and the preparation process of the base board is as follows: an adhesive is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed in a fixed mold at a pressure of 1 to 1.5 MPa for 10 minutes using a hot press.

[0018] As a preferred technical solution of the present invention, the decorative layer and the balancing layer are single-layer solid wood boards.

[0019] As a preferred technical solution of the present invention, in step S3, the dispersant is one of sodium lauryl sulfate and polyvinyl pyrrolidone.

[0020] As a preferred technical solution of the present invention, in step S4, the parameters of the electrostatic spraying are: static voltage of 60-80KV, spraying distance of 10-15cm, and leveling time of 5-15min.

[0021] As a preferred technical solution of the present invention, in step S7, the adhesive is a polyurethane adhesive.

[0022] As a preferred technical solution of the present invention, in step S7, the single-sided coating amount of the adhesive is 120-150 g / m 2 .

[0023] As a preferred technical solution of the present invention, in step S7, the hot pressing method is: assembling the composite floor by a hot press at a temperature of 160-180° C., a pressure of 0.2-0.5 MPa, and a time of 10-20 min.

[0024] As a preferred technical solution of the present invention, in step S7, the temperature of the heat preservation and pressure preservation is 130-150° C., the pressure is 0.1-0.4 MPa, and the time is 10 hours.

[0025] As a preferred technical solution of the present invention, the adhesive used in the substrate layer is diphenylmethane diisocyanate.

[0026] Beneficial effects of the present invention:

[0027] (1) In the present invention, nano titanium dioxide and mica iron oxide are used as fillers, and the corrosion-resistant coating is prepared by modification with polydopamine. The high chemical stability of nano titanium dioxide makes the coating more durable and can resist the erosion of environmental factors. At the same time, due to its special crystal structure, the iron oxide molecules are embedded in the mica crystals to form a unique layered structure, which makes the mica iron oxide have excellent chemical stability and corrosion resistance. In the coating, mica iron oxide can form a passivation film, which effectively inhibits the reaction of the coating surface to corrosion, thereby delaying the aging of the coating. Further, polydopamine can significantly improve the adhesion and durability of the coating by forming a thin film on the coating surface, effectively preventing the coating from peeling and falling off, thereby enhancing the corrosion resistance of the coating. In addition, the surface of polydopamine contains many functional groups (such as hydroxyl, amino, catechol, etc.), which can interact with nanomaterials, improve the compatibility of nanomaterials and coatings, and then add curcumin to increase the antioxidant property, which can improve the service life of the coating.

[0028] (2) Zirconia ceramics have excellent wear resistance because of their high hardness, high toughness and low friction coefficient. In addition, zirconia ceramics have higher density, finer texture and higher surface finish, which further reduces the friction coefficient and improves wear resistance. Modification with polyvinyl alcohol and sodium alginate increases the surface wettability of zirconia ceramics and improves their adhesion with other materials, which is conducive to better corrosion resistance. Silicon carbide is a high-performance abrasive with the characteristics of high hardness, high strength and high wear resistance. The large aspect ratio and small crystal size of calcium carbonate whiskers make it almost free of defects such as dislocations and grain boundaries that exist in general crystals. Therefore, its mechanical properties are close to those of complete crystals. When used as fillers, its reinforcing effect is very obvious and can effectively improve wear resistance. Through KH550 treatment, the three substances are dispersed more evenly, increasing their compatibility with the resin, which is conducive to better wear resistance. DETAILED DESCRIPTION

[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the present invention is further described in detail below in conjunction with embodiments.

[0030] Example 1

[0031] S1. In parts by weight, 10 parts of polyvinyl alcohol, 1 part of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics were ultrasonically mixed for 2 hours, and the temperature was raised to 80° C. and hot air dried to obtain modified zirconia ceramics;

[0032] 2 parts of stearic acid, 73 parts of aluminum oxide, 10 parts of modified zirconia ceramics, 10 parts of silicon carbide, and 5 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 hours, and fully mixed to prepare a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 4 hours at 40°C. After mixing, the solution was filtered out to obtain a modified filler;

[0033] S2, dispersing 10 parts of modified filler into 60 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer;

[0034] S3, ultrasonically dispersing 5 parts of nano titanium dioxide and 3 parts of mica iron oxide in 92 parts of deionized water, adding 1.5 parts of dopamine hydrochloride solution, and maintaining the solution pH at 8.0-9.0; stirring and reacting in a magnetic stirrer for 2 hours, then adding 0.5 parts of silane coupling agent, and continuing to stir and react at 80°C for 3 hours to obtain a polydopamine-modified nanofiller;

[0035] The mixture was put into a ball mill and fully ground at a speed of 300 r / min for 4 h, and sieved through 200 meshes to obtain nanofiller powder. 10 parts of nanofiller powder, 50 parts of polyvinyl alcohol, 30 parts of polyvinylidene fluoride resin, 5 parts of curcumin and 5 parts of sodium dodecyl sulfate were added to a reactor and mixed and stirred at a speed of 800 r / min for 2 h. The reaction temperature was 80°C to obtain a corrosion-resistant coating.

[0036] S4, grinding the surface of the wear-resistant layer to a thickness of 0.1 mm, spraying the corrosion-resistant coating on the ground surface of the wear-resistant layer by electrostatic spraying, wherein the voltage is 60 KV, the spraying distance is 10 cm, and the leveling time is 15 min;

[0037] S5, heating and curing the coating obtained in S4 at 160° C. for 2 hours to obtain the corrosion-resistant coating;

[0038] S6. Purging and drying each layer of the structure with nitrogen at 70°C;

[0039] S7. Diphenylmethane diisocyanate is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed in a fixed mold at a pressure of 1 MPa for 10 minutes using a hot press to obtain a base board, and the composite floor is assembled from bottom to top in the order of a balancing layer, an adhesive, a substrate layer, an adhesive, a decorative layer, an adhesive and a wear-resistant layer, wherein the decorative layer and the balancing layer are single-layer solid wood boards, and the composite floor is assembled by a hot press at a temperature of 160°C, a pressure of 0.2 MPa, and a time of 20 minutes, and the high corrosion-resistant and wear-resistant composite floor is prepared by heat-preserving and pressurizing at 130°C and 0.1 MPa for 10 hours, wherein the adhesive is a polyurethane adhesive, and the single-sided adhesive coating amount is 120 g / m 2 .

[0040] Example 2

[0041] S1. In parts by weight, 10 parts of polyvinyl alcohol, 1.5 parts of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics were ultrasonically mixed for 2 hours, and the temperature was raised to 60° C. and hot air dried to obtain modified zirconia ceramics;

[0042] 3 parts of stearic acid, 62 parts of aluminum oxide, 12 parts of modified zirconia ceramics, 15 parts of silicon carbide, and 8 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 hours, and fully mixed to obtain a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 4 hours at 50° C. After mixing, the solution was filtered out to obtain a modified filler.

[0043] S2, dispersing 15 parts of modified filler into 55 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer;

[0044] S3, ultrasonically dispersing 6 parts of nano titanium dioxide and 4 parts of mica iron oxide in 90 parts of deionized water, adding 1.5 parts of dopamine hydrochloride solution, and maintaining the solution pH at 8.0; stirring the reaction in a magnetic stirrer for 2 hours, then adding 0.8 parts of silane coupling agent, and continuing to stir the reaction at 80°C to obtain a polydopamine-modified nanofiller;

[0045] The mixture was put into a ball mill and fully ground at a speed of 300 r / min for 4 h, and sieved through 200 meshes to obtain nanofiller powder. 12 parts of nanofiller powder, 50 parts of polyvinyl alcohol, 30 parts of polyvinylidene fluoride resin, 4 parts of curcumin and 4 parts of sodium dodecyl sulfate were added to a reactor and mixed and stirred at a speed of 1000 r / min for 1 h. The reaction temperature was 70°C to obtain a corrosion-resistant coating.

[0046] S4, grinding the surface of the wear-resistant layer to a thickness of 0.2 mm, and spraying the corrosion-resistant coating on the ground wear-resistant layer surface by electrostatic spraying, wherein the voltage is 70 KV, the spraying distance is 12 cm, and the leveling time is 12 min;

[0047] S5, heating and curing the coating obtained in S4 at 170° C. for 1.5 h to obtain the corrosion-resistant coating;

[0048] S6. Purging and drying each layer of the structure with nitrogen at 70°C;

[0049] S7. Diphenylmethane diisocyanate is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed in a fixed mold at a pressure of 1.2 MPa for 10 minutes using a hot press to obtain a base board, and the composite floor is assembled from bottom to top in the order of a balancing layer, an adhesive, a substrate layer, an adhesive, a decorative layer, an adhesive and a wear-resistant layer, wherein the decorative layer and the balancing layer are single-layer solid wood boards, and the composite floor is assembled by a hot press at a temperature of 170°C, a pressure of 0.3 MPa, and a time of 15 minutes, and the high corrosion-resistant and wear-resistant composite floor is prepared by heat-preserving and pressurizing at 140°C and 0.2 MPa for 10 hours, wherein the adhesive is a polyurethane adhesive, and the single-sided adhesive coating amount is 130 g / m 2 .

[0050] Example 3

[0051] S1. In parts by weight, 10 parts of polyvinyl alcohol, 2 parts of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics were ultrasonically mixed for 2.5 hours, and the temperature was raised to 70° C. and hot air dried to obtain modified zirconia ceramics;

[0052] 4 parts of stearic acid, 60 parts of aluminum oxide, 15 parts of modified zirconia ceramics, 25 parts of silicon carbide, and 10 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 hours, and fully mixed to prepare a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 4 hours at 50° C. After mixing, the solution was filtered out to prepare a modified filler;

[0053] S2, dispersing 20 parts of modified filler into 50 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer;

[0054] S3, ultrasonically dispersing 8 parts of nano titanium dioxide and 5 parts of mica iron oxide in 87 parts of deionized water, adding 1.5 parts of dopamine hydrochloride solution, and maintaining the solution pH at 8.0; stirring the reaction in a magnetic stirrer for 2 hours, then adding 1 part of silane coupling agent, and continuing to stir the reaction at 80°C to obtain a polydopamine-modified nanofiller;

[0055] The mixture was put into a ball mill and fully ground at a speed of 300 r / min for 4 h, and sieved through 200 meshes to obtain nanofiller powder. 15 parts of nanofiller powder, 50 parts of polyvinyl alcohol, 30 parts of polyvinylidene fluoride resin, 4 parts of curcumin and 4 parts of sodium dodecyl sulfate were added to a reactor and mixed and stirred at a speed of 1000 r / min for 1 h. The reaction temperature was 70°C to obtain a corrosion-resistant coating.

[0056] S4, grinding the surface of the wear-resistant layer to a thickness of 0.3 mm, spraying the corrosion-resistant coating on the ground surface of the wear-resistant layer by electrostatic spraying, wherein the voltage is 80 KV, the spraying distance is 15 cm, and the leveling time is 5 min;

[0057] S5, heating and curing the coating obtained in S4 at 180° C. for 1 hour to obtain the corrosion-resistant coating;

[0058] S6. Purging and drying each layer of the structure with nitrogen at 70°C;

[0059] S7. Diphenylmethane diisocyanate is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed at a pressure of 1.5 MPa for 10 minutes in a fixed mold using a hot press to obtain a base board, and the composite floor is assembled from bottom to top in the order of balancing layer, adhesive, substrate layer, adhesive, decorative layer, adhesive and wear-resistant layer, and the decorative layer and the balancing layer are single-layer solid wood boards. The composite floor is assembled by a hot press at a temperature of 180°C, a pressure of 0.5 MPa, and a time of 10 minutes, and the high corrosion-resistant and wear-resistant composite floor is prepared by heat-preserving and pressurizing at 150°C and 0.4 MPa for 10 hours, wherein the adhesive is a mixture of melamine-modified urea-formaldehyde resin glue MUF and polyurethane adhesive in a mass ratio of 1:1, and the single-sided glue coating amount is 150g / m 2 .

[0060] Example 4

[0061] S1. In parts by weight, 10 parts of polyvinyl alcohol, 2 parts of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics were ultrasonically mixed for 3 hours, and the temperature was raised to 70° C. and hot air dried to obtain modified zirconia ceramics;

[0062] 4 parts of stearic acid, 60 parts of aluminum oxide, 15 parts of modified zirconia ceramics, 20 parts of silicon carbide, and 10 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 hours, and fully mixed to prepare a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 4 hours at 40°C. After mixing, the solution was filtered to obtain a modified filler;

[0063] S2, dispersing 20 parts of modified filler into 60 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer;

[0064] S3, ultrasonically dispersing 8 parts of nano titanium dioxide and 5 parts of mica iron oxide in 87 parts of deionized water, adding 1.5 parts of dopamine hydrochloride solution, and maintaining the solution pH at 9.0; stirring the reaction in a magnetic stirrer for 2 hours, and then adding 1 part of silane coupling agent, and continuing to stir the reaction at 75°C to obtain a polydopamine-modified nanofiller;

[0065] The mixture was put into a ball mill and fully ground at a speed of 300 r / min for 4 h, and sieved through 200 meshes to obtain nanofiller powder. 15 parts of nanofiller powder, 50 parts of polyvinyl alcohol, 30 parts of polyvinylidene fluoride resin, 2 parts of curcumin and 2 parts of polyvinyl pyrrolidone were added to a reactor and mixed and stirred at a speed of 900 r / min for 1.5 h. The reaction temperature was 75°C to obtain a corrosion-resistant coating.

[0066] S4, grinding the surface of the wear-resistant layer to a thickness of 0.3 mm, spraying the corrosion-resistant coating on the ground surface of the wear-resistant layer by electrostatic spraying, wherein the voltage is 80 KV, the spraying distance is 15 cm, and the leveling time is 5 min;

[0067] S5, heating and curing the coating obtained in S4 at 180° C. for 1 hour to obtain the corrosion-resistant coating;

[0068] S6. Purging and drying each layer of the structure with nitrogen at 70°C;

[0069] S7. Diphenylmethane diisocyanate is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed in a fixed mold at a pressure of 1.5 MPa for 10 minutes using a hot press to obtain a base board, and the composite floor is assembled from bottom to top in the order of a balancing layer, an adhesive, a substrate layer, an adhesive, a decorative layer, an adhesive and a wear-resistant layer, wherein the decorative layer and the balancing layer are single-layer solid wood boards, and the composite floor is assembled by a hot press at a temperature of 180°C, a pressure of 0.5 MPa, and a time of 10 minutes, and the high corrosion-resistant and wear-resistant composite floor is prepared by heat-preserving and pressurizing at 150°C and 0.4 MPa for 10 hours, wherein the adhesive is a polyurethane adhesive, and the single-sided adhesive coating amount is 150 g / m 2 .

[0070] Comparative Example 1

[0071] The difference between Comparative Example 1 and Example 1 is that the filler in the preparation of the wear-resistant layer is not modified by KH550, and the other operations are the same.

[0072] Comparative Example 2

[0073] The difference between Comparative Example 2 and Example 1 is that the zirconia ceramic is not modified when preparing the wear-resistant layer, and the other operations are the same.

[0074] Comparative Example 3

[0075] The difference between Comparative Example 3 and Example 1 is that silicon carbide is not added to the wear-resistant layer, and the other operations are the same.

[0076] Comparative Example 4

[0077] The difference between Comparative Example 4 and Example 1 is that no calcium carbonate whiskers are added to the wear-resistant layer, and the other operations are the same.

[0078] Comparative Example 5

[0079] The difference between Comparative Example 5 and Example 1 is that polydopamine is not used for modification in the corrosion-resistant coating, and the other operations are the same.

[0080] Corrosion resistant coating preparation:

[0081] 5 to 8 parts of nano titanium dioxide and 3 to 5 parts of mica iron oxide are put into a ball mill and fully ground at a speed of 300 r / min to make the particle size of the polydopamine-modified nano filler less than 10 μm to obtain a nano filler powder. 10 to 15 parts of nano filler powder, 40 to 50 parts of polyvinyl alcohol, 20 to 30 parts of polyvinylidene fluoride resin, 2 to 5 parts of curcumin and 2 to 5 parts of a dispersant are added into a reactor and mixed and stirred at a speed of 800 to 1000 r / min for 1 to 2 hours and a reaction temperature of 70 to 80° C. to obtain a corrosion-resistant coating.

[0082] Comparative Example 6

[0083] The difference between Comparative Example 6 and Example 1 is that nano titanium dioxide is not added to the corrosion-resistant coating, and the other operations are the same.

[0084] Comparative Example 7

[0085] The difference between Comparative Example 7 and Example 1 is that mica iron oxide is not added to the corrosion-resistant coating, and the other operations are the same.

[0086] Comparative Example 8

[0087] The difference between Comparative Example 8 and Example 1 is that curcumin is not used in the corrosion-resistant coating, and the other operations are the same.

[0088] 1. Wear resistance test

[0089] The wear resistance of the wear-resistant and corrosion-resistant composite floor prepared by the present invention was tested by using a JM-IV abrasion tester and a rotating friction rubber wheel method. The wear resistance of the present invention was measured by the average value of the coating mass loss (weight loss method) after 100 grinding revolutions. The load was 10N, the rotation speed was 80r / min, the test temperature was 25°C, the relative humidity was 50%, the mass was tested to an accuracy of 0.01mg, and the average value of 3 measurements was taken as the result. The test results are shown in Table 1.

[0090] Table 1

[0091]

[0092]

[0093] 2. Corrosion resistance test

[0094] Two thirds of the composite flooring prepared in Examples 1-4 and Comparative Examples 1-8 were immersed in 40°C water for 240 hours, and then dried to observe and record whether one side of the coating had gloss loss, discoloration, bubbles, wrinkles, or peeling, and to conduct a water resistance test.

[0095] 2 / 3 of the composite flooring prepared in Examples 1-4 and Comparative Examples 1-8 were immersed in a 25% by mass sodium chloride aqueous solution, a 5% by mass hydrochloric acid solution, and a 5% by mass sodium hydroxide aqueous solution for 48 hours, respectively. After drying, the coating was observed and recorded to see if there was any loss of gloss, discoloration, bubbles, wrinkles, or shedding on one side, and the salt resistance, acid resistance, and alkali resistance tests were performed.

[0096] The degree of corrosion is from large to small: partial detachment > small amount of bubbles > large amount of gloss loss, severe discoloration > small amount of gloss loss, slight discoloration > no gloss loss, no discoloration.

[0097] Through testing, it was found that after being immersed in four solvents, Examples 1-4 showed no gloss loss, no discoloration, bubbles, wrinkling, or shedding. Comparative Examples 1-4 and Comparative Example 8 showed a small amount of gloss loss and slight discoloration in the four solutions. Comparative Examples 5-7 showed a large amount of gloss loss in the aqueous solution, a small amount of bubbles in the salt solution, and partial shedding after being immersed in the acid and alkali solutions.

[0098] It can be seen from the above test data that the composite floor prepared by the present invention has excellent corrosion resistance and wear resistance.

[0099] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a highly corrosion-resistant and wear-resistant composite floor, the composite floor is composed of a wear-resistant layer, a decorative layer, a substrate layer, and a balancing layer from top to bottom, wherein the surface of the wear-resistant layer is coated with a corrosion-resistant coating, characterized in that: The specific preparation process of the composite floor is as follows: S1. In parts by weight, 10 parts of polyvinyl alcohol, 1-2 parts of sodium alginate, 50 parts of deionized water, 10 parts of ethanol and 25 parts of zirconia ceramics were mixed by ultrasonic for 2-3 h, and the temperature was raised to 60-80 °C and hot air dried to obtain modified zirconia ceramics; 2-4 parts of stearic acid, 60-75 parts of aluminum oxide, 10-15 parts of modified zirconia ceramics, 10-25 parts of silicon carbide, and 5-10 parts of calcium carbonate whiskers were ground by a ball mill at a speed of 300 r / min for 4 h, and fully mixed to obtain a filler. The filler was dispersed in a KH550 solution with a mass percentage of 15%, and fully stirred at a speed of 300 r / min for 3-4 h at 40-50 °C. After mixing, the solution was filtered to remove the modified filler. S2, dispersing 10-20 parts of modified filler into 50-60 parts of melamine formaldehyde resin, stirring evenly and then standing to solidify to obtain a wear-resistant layer; S3, ultrasonically disperse 5-8 parts of nano titanium dioxide and 3-5 parts of mica iron oxide in 70-100 parts of deionized water, add 1.5 parts of dopamine hydrochloride solution, and keep the solution pH at 8.0-9.0; stir and react in a magnetic stirrer for 1-2 h, then add 0.5-1 parts of silane coupling agent, and continue stirring and reacting at 70-80 °C for 3 h to obtain a polydopamine-modified nanofiller; The mixture was put into a ball mill and fully ground at a speed of 300 r / min for 4 h, and sieved through 200 meshes to obtain nanofiller powder. 10-15 parts of nanofiller powder, 40-50 parts of polyvinyl alcohol, 20-30 parts of polyvinylidene fluoride resin, 2-5 parts of curcumin and 2-5 parts of dispersant were added into a reactor, mixed and stirred at a speed of 800-1000 r / min for 1-2 h, and the reaction temperature was 70-80 °C to obtain a corrosion-resistant coating. S4, grinding the surface of the wear-resistant layer to a thickness of 0.1-0.3 mm, and spraying a corrosion-resistant coating on the ground surface of the wear-resistant layer by electrostatic spraying; S5, heating and curing the coating obtained in S4 at 160-180° C. for 1-2 h to obtain the corrosion-resistant coating; S6. Use nitrogen to purge and dry each layer of the structure at 70°C; S7, assembling the composite floor in the order of balancing layer, adhesive, substrate layer, adhesive, decorative layer, adhesive and wear-resistant layer from bottom to top by hot pressing at a temperature of 160-180 ° C and a pressure of 0.2-0.5 MPa for 10-20 min, and then keeping the temperature and pressure at a temperature of 130-150 ° C and a pressure of 0.1-0.4 MPa for 10 h to obtain the highly corrosion-resistant and wear-resistant composite floor; The substrate layer is a double-layer solid wood board, and the preparation process of the base board is as follows: an adhesive is applied between the double-layer solid wood boards, and the double-layer solid wood boards are hot-pressed in a fixed mold at a pressure of 1-1.5 MPa for 10 minutes using a hot press; The decorative layer and the balancing layer are single-layer solid wood boards.

2. The method for preparing the highly corrosion-resistant and wear-resistant composite floor according to claim 1, characterized in that: In step S3, the dispersant is one of sodium lauryl sulfate and polyvinyl pyrrolidone.

3. The method for preparing a highly corrosion-resistant and wear-resistant composite floor according to claim 1, characterized in that: In step S4, the parameters of the electrostatic spraying are: static voltage of 60-80 KV, spraying distance of 10-15 cm, and leveling time of 5-15 min.

4. The method for preparing a highly corrosion-resistant and wear-resistant composite floor according to claim 1, characterized in that: In step S7, the adhesive is a polyurethane adhesive.

5. The method for preparing the highly corrosion-resistant and wear-resistant composite floor according to claim 1, characterized in that: In step S7, the adhesive coating amount on one side is 120-150 g / m 2 .