Steel bar for automobile heat-resistant fastener and production process of steel bar

Through ECOARC ecological electric furnace smelting, LF furnace refining, RH refining, continuous casting, annealing, rolling and heat treatment processes, steel rods for automotive heat-resistant fasteners with excellent heat resistance and high mechanical properties were produced, and the current solution was solved. There are problems of insufficient heat resistance and mechanical properties of steel in the art, which improves the service life and safety of the automobile.

CN118957447AInactive Publication Date: 2024-11-15BENGANG STEEL PLATES CO LTD

Patent Information

Application Number
CN202411014068.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The heat resistance, mechanical properties and steel purity of existing steel for automotive fasteners are insufficient, which affects the service life and safety of the automobile.

Method used

The steel bars for automobile heat-resistant fasteners are produced using ECOARC ecological electric furnace smelting + LF furnace refining + RH refining + continuous casting + annealing + rolling + heat treatment processes to ensure that the chemical composition and mechanical properties of the steel meet the requirements of high-end products.

Benefits of technology

It realizes the high mechanical properties and high steel purity of steel rods for automotive heat-resistant fasteners, meets the surface quality and mechanical performance requirements of high-end products, and improves the service life and safety of the automobile.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965206970000121
    Figure BDA0004965206970000121
  • Figure BDA0004965206970000131
    Figure BDA0004965206970000131
  • Figure BDA0004965206970000132
    Figure BDA0004965206970000132
Patent Text Reader

Abstract

The invention discloses a steel bar for an automobile heat-resistant fastener and a production process thereof, and the steel bar comprises the following chemical components in percentage by mass: 0.23%-0.27% of C, 0.20%-0.35% of Si, 0.42%-0.60% of Mn, less than or equal to 0.015% of P, less than or equal to 0.012% of S, 1.52%-1.70% of Cr, less than or equal to 0.25% of Ni, 0.26%-0.33% of Mo, 0.16%-0.25% of V, less than or equal to 0.15% of Cu and the balance of Fe and inevitable impurities. The production process route comprises ecological electric furnace smelting, LF furnace refining, RH refining, continuous casting, annealing, heating furnace heating, rolling, heat preservation and heat treatment. The indexes such as the mechanical property and the high steel purity of the steel bar for the automobile heat-resistant fastener are guaranteed, the surface quality level of the steel bar for the automobile heat-resistant fastener is guaranteed, and the use requirement of the high-end automobile heat-resistant fastener is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special steel preparation, and in particular relates to a steel bar for automobile heat-resistant fasteners and a production process thereof. Background Art

[0002] As the basic parts of automobiles, there are many automotive fasteners, and they play a very important connecting role and even safety guarantee role in most positions. In recent years, my country's automobile manufacturing industry has developed rapidly, and industrial upgrading has been accelerating, which has put forward higher and higher requirements on the product quality and technical level of my country's automotive fastener industry. With the increasing demand for heat resistance, mechanical properties, fatigue life and steel purity of automotive fasteners, the quality of steel used for automotive heat-resistant fasteners directly affects the service life and wear resistance of the automobile, and even affects the safety of the entire automobile operation process. Therefore, research and development of automotive heat-resistant fastener steel with excellent heat resistance, mechanical properties and high steel purity has become an important topic that needs to be studied urgently. Summary of the invention

[0003] In view of this, the purpose of the present invention is to provide a steel bar for automobile heat-resistant fasteners and a production process thereof. The present invention adopts the process of ECOARC ecological electric furnace smelting + LF furnace refining + RH refining + continuous casting + annealing + rolling + heat treatment to produce steel bars for automobile heat-resistant fasteners, which not only ensures the mechanical properties of the finished steel and high steel purity of the steel bars for automobile heat-resistant fasteners, but also ensures the surface quality level of the steel bars for automobile heat-resistant fasteners, and realizes a breakthrough in the batch production of steel bars for automobile heat-resistant fasteners by the ecological electric furnace continuous casting process, meeting the use requirements of high-end automobile heat-resistant fasteners.

[0004] In order to achieve the above object, the present invention provides the following technical solutions:

[0005] The invention provides a steel bar for automobile heat-resistant fasteners. The chemical composition and mass percentage of the steel bar for automobile heat-resistant fasteners are as follows: C: 0.23%-0.27%, Si: 0.20%-0.35%, Mn: 0.42%-0.60%, P: ≤0.015%, S: ≤0.012%, Cr: 1.52%-1.70%, Ni: ≤0.25%, Mo: 0.26%-0.33%, V: 0.16%-0.25%, Cu: ≤0.15%, and the balance is Fe and unavoidable impurities.

[0006] The present invention also provides a production process for the above-mentioned steel bars for automobile heat-resistant fasteners, and the production process route is as follows: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating in a heating furnace → rolling → insulation → heat treatment;

[0007] ECOARC ecological electric furnace smelting process, tapping temperature 1600 ~ 1610 ℃, C 0.08 ~ 0.10%, P ≤ 0.010%, tapping volume 106 ~ 113t, smelting cycle 35 ~ 45min;

[0008] LF furnace refining process, LF inlet temperature is 1540~1550℃, and molten steel leaves the station when the temperature reaches 1640~1650℃, and LF smelting cycle is 60min~70min;

[0009] RH refining process, the inlet temperature is 1580-1590℃, the argon pressure is controlled before the vacuum pump is started so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 100-110Pa, the timing starts, and the holding time is 10-15min. Argon is blown statically, the outlet temperature is 1580-1590℃, and the operation time is 40min-50min.

[0010] In the continuous casting process, the temperature of the ladle at the station is 1565-1575℃, the amount of molten steel is 95-105t, the H in the tundish is controlled to be ≤2ppm, the whole process is protected casting, and the mold protection slag uses medium carbon steel protection slag;

[0011] Annealing process, annealing temperature 640 ~ 650 ℃, annealing time 30 ~ 35h, furnace temperature ≤ 200 ℃.

[0012] Heating process of heating furnace: the temperature of entering heating furnace is 450℃~560℃, the temperature of soaking section is controlled at 1190℃~1210℃, the time is 1.3~1.5h; the steel tapping temperature is 1185℃~1195℃;

[0013] Rolling process, initial rolling temperature 1000 ~ 1050 ℃, final rolling temperature 800 ~ 900 ℃;

[0014] Insulation process, the temperature of the lower insulation pit is 550~590℃, insulation is 50~55h, and the exit temperature is ≤180℃.

[0015] Based on the above technical solution, further, in the ECOARC ecological electric furnace smelting process, slag, pre-deoxidizer, and ferroalloy are added when 1 / 4 to 1 / 3 of the steel is tapped. The amount of alloy added per ton of steel is: 5.0 to 5.2 kg / t of silicon manganese, 10 to 10.5 kg / t of high carbon ferrochrome, 16 to 16.5 kg / t of low carbon ferrochrome, and 1.0 to 1.2 kg / t of aluminum wire segment (10-16 mm). The amount of auxiliary materials added per ton of steel is: 40 to 41 kg / t of active lime (10-70 mm), 25 to 26 kg / t of magnesite (10-60 mm), 6 to 6.2 kg / t of ladle ash, 20 to 21 kg / t of small coke pieces, and 18 to 19 kg / t of coking CDQ powder.

[0016] Based on the above technical solution, further, the ECOARC ecological electric furnace smelting process, the smelting raw materials include 38-45t of molten iron, 20-21t of alloy structural steel heads, 43-45t of heavy scrap steel, and 10-11t of lump-type scrap steel.

[0017] Based on the above technical scheme, further, in the LF furnace refining process, after the LF enters the station, a large current of 35000~36000A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and the arc are not exposed, active lime is added. After 5~6 minutes, the chemical composition is analyzed for the first time, and alloys are added according to the target value of the chemical composition, and carbon is increased to promote rapid melting and homogenization of the alloy and carbon powder; when the temperature of the molten steel reaches 1600~1610℃, 1.5~1.6kg / t of diffusion deoxidizer alumina balls are added for diffusion deoxidation, and the furnace door is closed for 10~13min. When the temperature of the molten steel reaches 1620~1630℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value.

[0018] Based on the above technical scheme, further, in the LF furnace refining process, the additional alloys include: ferrosilicon 1.1-1.2 kg / t, high carbon ferromanganese 2.1-2.2 kg / t, high carbon ferrochrome 3.9-4.0 kg / t, ferromolybdenum 0.4-0.5 kg / t, ferrovanadium (FeV50-B) 3.5-3.6 kg / t, aluminum wire (Φ10-Φ12 mm) 1-1.1 m / t; additional auxiliary materials: active lime (10-70 mm) 4-4.2 kg / t, silicon carbide (1-5 mm) 2.1-2.2 kg / t, and coke particles 0.75-0.80 kg / t.

[0019] Based on the above technical solution, further, in the RH refining process, the argon pressure is controlled at 0.1-0.3MPa before the vacuum pump is started, and the argon pressure is adjusted to 0.3-0.5MPa during the static argon blowing process. After the static argon blowing is completed, 2-2.1 meters / t of silicon-calcium alloy cored wire (Φ14-Φ14.2mm) and 0.6-0.7kg / t of covering agent are added.

[0020] Based on the above technical solution, further, in the heating process of the heating furnace, the temperature of the preheating section is controlled at 660℃~700℃, and the time is 1.3~1.5h; the temperature of the heating section 2 is controlled at 850℃~860℃, and the time is 1.3~1.5h; the temperature of the heating section 1 is controlled at 1190℃~1220℃, and the time is 1.3~1.5h.

[0021] Based on the above technical solution, further, the rolling process, the continuous casting billet initial rolling process: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 64.9 ~ 65.1mm → 2nd pass reduction 69.9 ~ 70.1mm → steel turning → 3rd pass reduction 63.9 ~ 64.1mm → 4th pass reduction 89.9 ~ 90.1mm → steel turning → 5th pass reduction 41.9 ~ 42.1mm → 6th pass reduction 39.9 ~ 40.1mm → 7th pass reduction 34.9 ~ 35.1mm → 8th pass reduction 33.9 ~ 34.1mm → steel turning → 9th pass reduction 81.9 ~ 82.1mm, through 3 850mm rolling mills, 1 735mm rolling mill, and then enter the 8-frame continuous rolling mill group for rolling;

[0022] Rolling process: 8 passes, the first pass is 228.9-229.1mm high and 244.9-245.1mm wide; the second pass is 191.9-192.1mm high and 234.9-235.1mm wide; the third pass is 199.9-200.1mm high and 194.9-195.1mm wide; the fourth pass is 168.9-169.1mm high and 212.7-212.9mm wide mm; the 5th pass is 176.9~177.1mm high and 179.9~180.1mm wide; the 6th pass is 140.9~141.1mm high and 191.9~192.1mm wide; the 7th pass is 151.9~152.1mm high and 151.9~152.1mm wide; the 8th pass is 151.9~152.1mm high and 151.9~152.1mm wide; the finished product is produced after 8 passes.

[0023] Based on the above technical solution, further, the heat treatment process includes the following steps:

[0024] 1) Quenching: 890-910°C, insulation 0.9-1.2h, oil cooling;

[0025] 2) Tempering: 630-650℃, keep warm for 1.9-2.2h, air cooling.

[0026] The beneficial effects of the present invention compared with the prior art are as follows:

[0027] (1) The present invention adopts 100t ECOARC ecological electric furnace + LF + RH + 390mm*480mm continuous casting, rolling and heat treatment process to produce steel bars for automotive heat-resistant fasteners. The production specification is Φ150mm, which meets the mechanical property requirements and ensures the purity of the steel.

[0028] (2) The reasonable composition design and production process of the present invention ensure the surface quality and mechanical properties of the steel bars for automotive heat-resistant fasteners.

[0029] (3) The finished steel macrostructure and non-metallic inclusions of the steel bar for automobile heat-resistant fasteners prepared by the present invention meet the requirements of high-end products. DETAILED DESCRIPTION

[0030] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.

[0031] Embodiment 1:

[0032] This embodiment provides a production process for steel bars for automotive heat-resistant fasteners, and the specific process is as follows:

[0033] The chemical composition and mass percentage of steel bars for automotive heat-resistant fasteners are as follows: C: 0.25%, Si: 0.26%, Mn: 0.48%, P: 0.011%, S: 0.006%, Cr: 1.59%, Ni: 0.05%, Mo: 0.28%, V: 0.19%, Cu: 0.05%, and the balance is Fe and unavoidable impurities.

[0034] Process route: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment → finishing → inspection → packaging and storage → delivery;

[0035] (1) Ecological electric furnace smelting

[0036] The amount of molten iron charged is 42t; the amount of scrap steel charged is: 20t of alloy structural steel cutting head, 44t of heavy scrap steel, 10t of lump scrap steel; the tapping temperature is 1605℃, C is 0.09% and P is 0.008% when tapping, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 of the steel is tapped, the amount of steel tapped is 109t, and the smelting cycle is 40min. The amount of alloy added per ton of steel is: 5.1Kg / t of silicon manganese, 10.2Kg / t of high carbon ferrochrome, 16Kg / t of low carbon ferrochrome, 1.1Kg / t of aluminum wire segment (10mm). The amount of auxiliary materials added per ton of steel is: 40Kg / t of active lime (35mm), 25Kg / t of magnesite (40mm), 6Kg / t of ladle ash, 20Kg / t of small coke block, and 18Kg / t of coking CDQ powder.

[0037] (2) LF furnace refining

[0038] The LF station temperature is 1545℃, and a large current of 35600A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and arc are not exposed, active lime is added. The chemical composition is analyzed for the first time after 5 minutes. Alloy is added according to the target value of the chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1605℃, 1.5kg / t of alumina balls as diffusion deoxidizer are added for diffusion deoxidation. The furnace door is closed for 11 minutes. When the temperature of the molten steel reaches 1626℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value. After the second sample is taken, the station is left when the temperature of the molten steel reaches 1645℃. The LF smelting cycle is 65 minutes. The alloys are added: 1.1kg / t of ferrosilicon, 2.1kg / t of high carbon ferromanganese, 3.9kg / t of high carbon ferrochrome, 0.45kg / t of ferromolybdenum, 3.5kg / t of ferrovanadium (FeV50-B), 1.0m / t of aluminum wire (Φ10mm). Supplementary materials: 4kg / t of active lime (35mm), 2.1kg / t of silicon carbide (3mm), and 0.77kg / t of coke particles.

[0039] (3) RH refining

[0040] The inlet temperature is 1586℃, the operation time is 46min, and the argon pressure is controlled at 0.1MPa before the vacuum pump is started, so that the slag surface moves slightly and the molten steel is not exposed. When the vacuum degree reaches 100Pa, the timing starts and the maintenance time is 12min. At the same time, the argon pressure is adjusted to 0.3MPa. After the static argon blowing is completed, 2.0m / t of silicon-calcium alloy cored wire (Φ14mm) and 0.6kg / t of covering agent are added. The outlet temperature is 1587℃.

[0041] (4) Continuous casting

[0042] The temperature of the ladle arriving at the station is 1570℃, the amount of molten steel is 98t, the H content of the tundish is controlled at 1.5ppm, the casting is protected throughout the whole process, and the crystallizer protection slag uses medium carbon steel protection slag.

[0043] (5) Annealing

[0044] Continuous casting slab annealing, annealing temperature 646 ℃, annealing time 33h, furnace temperature 160 ℃.

[0045] (6) Heating process

[0046] Heating process: the temperature entering the heating furnace is 490℃, the temperature of the preheating section is required to be 680℃, and the time is 1.3h; the temperature of the heating section 2 is required to be 854℃, and the time is 1.3h; the temperature of the heating section 1 is required to be 1205℃, and the time is 1.5h; the temperature of the soaking section is required to be 1200℃, and the time is 1.3h; the steel tapping temperature is 1190℃.

[0047] (7) Rolling process

[0048] Initial rolling temperature is 1050℃, final rolling temperature is 880℃;

[0049] Continuous casting slab initial rolling process: 9 rolling passes, rolling reduction: steel turning → 1st pass reduction 65mm → 2nd pass reduction 70mm → steel turning → 3rd pass reduction 64mm → 4th pass reduction 90mm → steel turning → 5th pass reduction 42mm → 6th pass reduction 40mm → 7th pass reduction 35mm → 8th pass reduction 34mm → steel turning → 9th pass reduction 82mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering 8-stand continuous rolling mill group for rolling;

[0050] Rolling process of the produced material: 8 rolling passes, the 1st pass is 229mm high and 245mm wide; the 2nd pass is 192mm high and 235mm wide; the 3rd pass is 200mm high and 195mm wide; the 4th pass is 169mm high and 212.8mm wide; the 5th pass is 177mm high and 180mm wide; the 6th pass is 141mm high and 192mm wide; the 7th pass is 152mm high and 152mm wide; the 8th pass is 152mm high and 152mm wide; the finished product is produced after 8 passes.

[0051] (8) Insulation process

[0052] Insulation process: Steel insulation, lower insulation pit temperature 590℃, insulation 53h, exit pit temperature 150℃.

[0053] (9) Heat treatment process

[0054] The steel after heat preservation is heat treated, and the heat treatment includes the following steps:

[0055] 1) Quenching: 900℃, holding time 1.0h, oil cooling;

[0056] 2) Tempering: 640℃, keep warm for 2.0h, air cool.

[0057] Embodiment 2:

[0058] This embodiment provides a production process for steel bars for automotive heat-resistant fasteners, and the specific process is as follows:

[0059] The chemical composition and mass percentage of steel bars for automotive heat-resistant fasteners are as follows: C: 0.24%, Si: 0.26%, Mn: 0.49%, P: 0.012%, S: 0.006%, Cr: 1.59%, Ni: 0.05%, Mo: 0.28%, V: 0.20%, Cu: 0.05%, and the balance is Fe and unavoidable impurities.

[0060] Process route: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment → finishing → inspection → packaging and storage → delivery;

[0061] (1) Ecological electric furnace smelting

[0062] The amount of molten iron charged is 42t; the amount of scrap steel charged is: 20t of alloy structural steel cutting head, 44t of heavy scrap steel, 10t of lump scrap steel; the tapping temperature is 1606℃, the C is 0.08% and the P is 0.008% when tapping, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 of the steel is tapped, the amount of steel tapped is 109t, and the smelting cycle is 40min. The amount of alloy added per ton of steel is: 5.1Kg / t of silicon manganese, 10Kg / t of high carbon ferrochrome, 16.2Kg / t of low carbon ferrochrome, 1.1Kg / t of aluminum wire segment (10mm). The amount of auxiliary materials added per ton of steel is: 40Kg / t of active lime (35mm), 25Kg / t of magnesite (40mm), 6.0Kg / t of ladle ash, 20Kg / t of small coke block, and 18Kg / t of coking CDQ powder.

[0063] (2) LF furnace refining

[0064] The LF station temperature is 1545℃, and a large current of 35500A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and arc are not exposed, active lime is added. The chemical composition is analyzed for the first time after 5 minutes. Alloy is added according to the target value of the chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1603℃, 1.5kg / t of alumina balls as diffusion deoxidizer are added for diffusion deoxidation, and the furnace door is closed for 11 minutes. When the temperature of the molten steel reaches 1625℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value. After the second sample is taken, the station is left when the temperature of the molten steel reaches 1646℃. The LF smelting cycle is 64 minutes. The alloys are added: 1.1kg / t of ferrosilicon, 2.1kg / t of high carbon ferromanganese, 3.9kg / t of high carbon ferrochrome, 0.45kg / t of ferromolybdenum, 3.5kg / t of ferrovanadium (FeV50-B), 1.0m / t of aluminum wire (Φ10mm). Supplementary materials: 4.0Kg / t of active lime (35mm), 2.1kg / t of silicon carbide (5mm), and 0.77kg / t of coke particles.

[0065] (3) RH refining

[0066] The inlet temperature is 1585℃, the operation time is 46min, and the argon pressure is controlled at 0.1MPa before the vacuum pump is started, so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 105Pa, the timing starts and the time is maintained for 12min. At the same time, the argon pressure is adjusted to 0.3MPa. After the static argon blowing is completed, 2.0m / t of silicon-calcium alloy cored wire (Φ14mm) and 0.6kg / t of covering agent are added. The outlet temperature is 1586℃.

[0067] (4) Continuous casting

[0068] The temperature of the ladle arriving at the station is 1570℃, the amount of molten steel is 98t, the H content of the tundish is controlled at 1.4ppm, the casting is protected throughout the whole process, and the crystallizer protection slag uses medium carbon steel protection slag.

[0069] (5) Annealing

[0070] Continuous casting slab annealing, annealing temperature 647 ℃, annealing time 32h, furnace temperature 160 ℃.

[0071] (6) Heating process

[0072] Heating process: the temperature entering the heating furnace is 520℃, the temperature of the preheating section is required to be 680℃, and the time is 1.4h; the temperature of the heating section 2 is required to be 854℃, and the time is 1.4h; the temperature of the heating section 1 is required to be 1198℃, and the time is 1.5h; the temperature of the soaking section is required to be 1200℃, and the time is 1.3h; the steel tapping temperature is 1190℃.

[0073] (7) Rolling process

[0074] Initial rolling temperature is 1020℃, final rolling temperature is 855℃;

[0075] The initial rolling process of continuous casting slab: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 65mm → 2nd pass reduction 70mm → steel turning → 3rd pass reduction 64mm → 4th pass reduction 90mm → steel turning → 5th pass reduction 42mm → 6th pass reduction 40mm → 7th pass reduction 35mm → 8th pass reduction 34mm → steel turning → 9th pass reduction 82mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering the 8-pass continuous rolling unit for rolling.

[0076] Rolling process of the produced material: 8 rolling passes, the 1st pass is 229mm high and 245mm wide; the 2nd pass is 192mm high and 235mm wide; the 3rd pass is 200mm high and 195mm wide; the 4th pass is 169mm high and 212.8mm wide; the 5th pass is 177mm high and 180mm wide; the 6th pass is 141mm high and 192mm wide; the 7th pass is 152mm high and 152mm wide; the 8th pass is 152mm high and 152mm wide; the finished product is produced after 8 passes.

[0077] (8) Insulation process

[0078] Insulation process: Steel insulation, lower insulation pit temperature 570℃, insulation 53h, exit pit temperature 150℃.

[0079] (9) Heat treatment process

[0080] The steel after heat preservation is heat treated, and the heat treatment includes the following steps:

[0081] 1) Quenching: 900℃, holding time 1.0h, oil cooling;

[0082] 2) Tempering: 640℃, keep warm for 2.0h, air cool.

[0083] Embodiment 3:

[0084] This embodiment provides a production process for steel bars for automotive heat-resistant fasteners, and the specific process is as follows:

[0085] The chemical composition and mass percentage of steel bars for automotive heat-resistant fasteners are as follows: C: 0.25%, Si: 0.26%, Mn: 0.50%, P: 0.010%, S: 0.005%, Cr: 1.60%, Ni: 0.05%, Mo: 0.28%, V: 0.20%, Cu: 0.05%, and the balance is Fe and unavoidable impurities.

[0086] Process route: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment → finishing → inspection → packaging and storage → delivery;

[0087] (1) Ecological electric furnace smelting

[0088] The amount of molten iron charged is 41t; the amount of scrap steel charged is: 20t of alloy structural steel cutting head, 44t of heavy scrap steel, 10t of lump scrap steel; the tapping temperature is 1607℃, the C is 0.08% and the P is 0.009% when tapping, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 of the steel is tapped, the tapping amount is 110t, and the smelting cycle is 39min. The amount of alloy added per ton of steel is: 5.1Kg / t of silicon manganese, 10Kg / t of high carbon ferrochrome, 16Kg / t of low carbon ferrochrome, 1.1Kg / t of aluminum wire segment (10mm). The amount of auxiliary materials added per ton of steel is: 40Kg / t of active lime (35mm), 25Kg / t of magnesite (40mm), 6.1Kg / t of ladle ash, 20Kg / t of small coke block, and 18Kg / t of coking CDQ powder.

[0089] (2) LF furnace refining

[0090] The LF station temperature is 1545℃, and a large current of 35700A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and arc are not exposed, active lime is added. The chemical composition is analyzed for the first time after 5 minutes. Alloy is added according to the target value of the chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1603℃, 1.5kg / t of alumina balls as diffusion deoxidizer are added for diffusion deoxidation, and the furnace door is closed for 11 minutes. When the temperature of the molten steel reaches 1625℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value. After the second sample is taken, the station is left when the temperature of the molten steel reaches 1644℃. The LF smelting cycle is 67 minutes. The alloys are added: 1.1kg / t of ferrosilicon, 2.1kg / t of high carbon ferromanganese, 3.9kg / t of high carbon ferrochrome, 0.44kg / t of ferromolybdenum, 3.5kg / t of ferrovanadium (FeV50-B), 1.1m / t of aluminum wire (Φ10mm). Supplementary materials: 4.0Kg / t of active lime (35mm), 2.1kg / t of silicon carbide (5mm), and 0.78kg / t of coke particles.

[0091] (3) RH refining

[0092] The inlet temperature is 1584℃, the operation time is 48min, and the argon pressure is controlled at 0.1MPa before the vacuum pump is started, so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 103Pa, the timing starts and the time is maintained for 12min. At the same time, the argon pressure is adjusted to 0.4MPa. After the static argon blowing is completed, 2.0m / t of silicon-calcium alloy cored wire (Φ14mm) and 0.6kg / t of covering agent are added. The outlet temperature is 1586℃.

[0093] (4) Continuous casting

[0094] The temperature of the ladle arriving at the station is 1570℃, the amount of molten steel is 101t, the H content of the tundish is controlled at 1.4ppm, the casting is protected throughout the whole process, and the crystallizer protection slag uses medium carbon steel protection slag.

[0095] (5) Annealing

[0096] Continuous casting slab annealing, annealing temperature 645 ℃, annealing time 32h, furnace temperature 140 ℃.

[0097] (6) Heating process

[0098] Heating process: the temperature entering the heating furnace is 500℃, the temperature of the preheating section is required to be 680℃, and the time is 1.3h; the temperature of the heating section 2 is required to be 854℃, and the time is 1.4h; the temperature of the heating section 1 is required to be 1195℃, and the time is 1.5h; the temperature of the soaking section is required to be 1198℃, and the time is 1.3h; the steel tapping temperature is 1190℃.

[0099] (7) Rolling process

[0100] Initial rolling temperature 1010℃, final rolling temperature 835℃;

[0101] The initial rolling process of continuous casting slab: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 65mm → 2nd pass reduction 70mm → steel turning → 3rd pass reduction 64mm → 4th pass reduction 90mm → steel turning → 5th pass reduction 42mm → 6th pass reduction 40mm → 7th pass reduction 35mm → 8th pass reduction 34mm → steel turning → 9th pass reduction 82mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering the 8-pass continuous rolling unit for rolling.

[0102] Rolling process of the produced material: 8 rolling passes, the 1st pass is 229mm high and 245mm wide; the 2nd pass is 192mm high and 235mm wide; the 3rd pass is 200mm high and 195mm wide; the 4th pass is 169mm high and 212.8mm wide; the 5th pass is 177mm high and 180mm wide; the 6th pass is 141mm high and 192mm wide; the 7th pass is 152mm high and 152mm wide; the 8th pass is 152mm high and 152mm wide; the finished product is produced after 8 passes.

[0103] (8) Insulation process

[0104] Insulation process: Steel insulation, lower insulation pit temperature 570℃, insulation 52h, exit pit temperature 160℃.

[0105] (9) Heat treatment process

[0106] The steel after heat preservation is heat treated, and the heat treatment includes the following steps:

[0107] 1) Quenching: 900℃, holding time 1.0h, oil cooling;

[0108] 2) Tempering: 640℃, keep warm for 2.0h, air cool.

[0109] Embodiment 4:

[0110] This embodiment provides a production process for steel bars for automotive heat-resistant fasteners, and the specific process is as follows:

[0111] The chemical composition and mass percentage of steel bars for automotive heat-resistant fasteners are as follows: C: 0.24%, Si: 0.26%, Mn: 0.49%, P: 0.011%, S: 0.006%, Cr: 1.59%, Ni: 0.05%, Mo: 0.30%, V: 0.19%, Cu: 0.05%, and the balance is Fe and unavoidable impurities.

[0112] Process route: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment → finishing → inspection → packaging and storage → delivery;

[0113] (1) Ecological electric furnace smelting

[0114] The amount of molten iron charged is 43t; the amount of scrap steel charged is: 20t of alloy structural steel cutting head, 44t of heavy scrap steel, 10t of lump scrap steel; the tapping temperature is 1606℃, the C is 0.09% and the P is 0.008% when tapping, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 of the steel is tapped, the amount of steel tapped is 109t, and the smelting cycle is 40min. The amount of alloy added per ton of steel is: 5.1Kg / t of silicon manganese, 10.2Kg / t of high carbon ferrochrome, 16Kg / t of low carbon ferrochrome, and 1.1Kg / t of aluminum wire segment (10-16mm). The amount of auxiliary materials added per ton of steel is: 40Kg / t of active lime (35mm), 25Kg / t of magnesite (40mm), 6.0Kg / t of ladle ash, 20Kg / t of small coke block, and 18Kg / t of coking CDQ powder.

[0115] (2) LF furnace refining

[0116] The LF station temperature is 1547℃, and a large current of 35700A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and arc are not exposed, active lime is added. The chemical composition is analyzed for the first time after 5 minutes. Alloy is added according to the target value of the chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1605℃, 1.5kg / t of alumina balls as diffusion deoxidizer are added for diffusion deoxidation, and the furnace door is closed for 11 minutes. When the temperature of the molten steel reaches 1625℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value. After the second sample is taken, the station is left when the temperature of the molten steel reaches 1648℃. The LF smelting cycle is 63 minutes. The alloys are added: 1.1kg / t of ferrosilicon, 2.1kg / t of high carbon ferromanganese, 3.9kg / t of high carbon ferrochrome, 0.43kg / t of ferromolybdenum, 3.5kg / t of ferrovanadium (FeV50-B), and 1.0m / t of aluminum wire (Φ10mm). Supplementary materials: 4.1Kg / t of active lime (35mm), 2.1kg / t of silicon carbide (5mm), and 0.77kg / t of coke particles.

[0117] (3) RH refining

[0118] The inlet temperature is 1586℃, the operation time is 48min, and the argon pressure is controlled at 0.1MPa before the vacuum pump is started, so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 103Pa, the timing starts and the time is maintained for 12min. At the same time, the argon pressure is adjusted to 0.3MPa. After the static argon blowing is completed, 2.0m / t of silicon-calcium alloy cored wire (Φ14mm) and 0.6kg / t of covering agent are added. The outlet temperature is 1585℃.

[0119] (4) Continuous casting

[0120] The temperature of the ladle arriving at the station is 1571℃, the amount of molten steel is 98t, the H content of the tundish is controlled at 1.5ppm, the casting is protected throughout the whole process, and the crystallizer protection slag uses medium carbon steel protection slag.

[0121] (5) Annealing

[0122] Continuous casting slab annealing, annealing temperature 645 ℃, annealing time 33h, furnace temperature 160 ℃.

[0123] (6) Heating process

[0124] Heating process: the temperature entering the heating furnace is 520℃, the temperature of the preheating section is required to be 680℃, and the time is 1.3h; the temperature of the heating section 2 is required to be 854℃, and the time is 1.3h; the temperature of the heating section 1 is required to be 1198℃, and the time is 1.3h; the temperature of the soaking section is required to be 1200℃, and the time is 1.3h; the steel tapping temperature is 1190℃.

[0125] (7) Rolling process

[0126] Initial rolling temperature is 1030℃, final rolling temperature is 860℃;

[0127] The initial rolling process of continuous casting slab: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 65mm → 2nd pass reduction 70mm → steel turning → 3rd pass reduction 64mm → 4th pass reduction 90mm → steel turning → 5th pass reduction 42mm → 6th pass reduction 40mm → 7th pass reduction 35mm → 8th pass reduction 34mm → steel turning → 9th pass reduction 82mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering the 8-pass continuous rolling unit for rolling.

[0128] Rolling process of the produced material: 8 rolling passes, the 1st pass is 229mm high and 245mm wide; the 2nd pass is 192mm high and 235mm wide; the 3rd pass is 200mm high and 195mm wide; the 4th pass is 169mm high and 212.8mm wide; the 5th pass is 177mm high and 180mm wide; the 6th pass is 141mm high and 192mm wide; the 7th pass is 152mm high and 152mm wide; the 8th pass is 152mm high and 152mm wide; the finished product is produced after 8 passes.

[0129] (8) Insulation process

[0130] Insulation process: Steel insulation, lower insulation pit temperature 580℃, insulation 52h, exit pit temperature 150℃.

[0131] (9) Heat treatment process

[0132] The steel after heat preservation is heat treated, and the heat treatment includes the following steps:

[0133] 1) Quenching: 900℃, holding time 1.0h, oil cooling;

[0134] 2) Tempering: 640℃, keep warm for 2.0h, air cool.

[0135] Embodiment 5:

[0136] This embodiment provides a production process for steel bars for automotive heat-resistant fasteners, and the specific process is as follows:

[0137] The chemical composition and mass percentage of steel bars for automotive heat-resistant fasteners are as follows: C: 0.25%, Si: 0.27%, Mn: 0.48%, P: 0.012%, S: 0.005%, Cr: 1.60%, Ni: 0.05%, Mo: 0.30%, V: 0.20%, Cu: 0.05%, and the balance is Fe and unavoidable impurities.

[0138] Process route: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment → finishing → inspection → packaging and storage → delivery;

[0139] (1) Ecological electric furnace smelting

[0140] The amount of molten iron charged is 42t; the amount of scrap steel charged is: 20t of alloy structural steel cutting head, 44t of heavy scrap steel, 10t of lump scrap steel; the tapping temperature is 1605℃, the C is 0.08% and the P is 0.009% when tapping, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 of the steel is tapped, the tapping amount is 110t, and the smelting cycle is 40min. The amount of alloy added per ton of steel is: 5.1Kg / t of silicon manganese, 10.0Kg / t of high carbon ferrochrome, 16Kg / t of low carbon ferrochrome, 1.1Kg / t of aluminum wire segment (10mm). The amount of auxiliary materials added per ton of steel is: 40Kg / t of active lime (35mm), 25Kg / t of magnesite (40mm), 6.0Kg / t of ladle ash, 20Kg / t of small coke block, and 18Kg / t of coking CDQ powder.

[0141] (2) LF furnace refining

[0142] The LF station temperature is 1545℃, and a large current of 35800A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and arc are not exposed, active lime is added. The chemical composition is analyzed for the first time after 5 minutes. Alloy is added according to the target value of the chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1605℃, 1.5kg / t of alumina balls as diffusion deoxidizer are added for diffusion deoxidation, and the furnace door is closed for 11 minutes. When the temperature of the molten steel reaches 1625℃, the chemical composition is analyzed for the second time to confirm the deviation of the content of each chemical element from the target value. After the second sample is taken, the station is left when the temperature of the molten steel reaches 1645℃. The LF smelting cycle is 65 minutes. The alloys are added: 1.1kg / t of ferrosilicon, 2.1kg / t of high carbon ferromanganese, 3.9kg / t of high carbon ferrochrome, 0.4kg / t of ferromolybdenum, 3.5kg / t of ferrovanadium (FeV50-B), and 1.0m / t of aluminum wire (Φ10mm). Supplementary materials: 4.0Kg / t of active lime (35mm), 2.1kg / t of silicon carbide (5mm), and 0.77kg / t of coke particles.

[0143] (3) RH refining

[0144] The inlet temperature is 1586℃, the operation time is 45min, and the argon pressure is controlled at 0.1MPa before the vacuum pump is started, so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 104Pa, the timing starts and the maintenance time is 12min. At the same time, the argon pressure is adjusted to 0.3MPa. After the static argon blowing is completed, 2.0m / t of silicon-calcium alloy cored wire (Φ14mm) and 0.6kg / t of covering agent are added. The outlet temperature is 1588℃.

[0145] (4) Continuous casting

[0146] The temperature of the ladle arriving at the station is 1572℃, the amount of molten steel is 102t, the H content of the tundish is controlled at 1.4ppm, the casting is protected throughout the whole process, and the crystallizer protection slag uses medium carbon steel protection slag.

[0147] (5) Annealing

[0148] Continuous casting slab annealing, annealing temperature 645 ℃, annealing time 32h, furnace temperature 170 ℃.

[0149] (6) Heating process

[0150] Heating process: the temperature entering the heating furnace is 520℃, the temperature of the preheating section is required to be 670℃, and the time is 1.4h; the temperature of the heating section 2 is required to be 855℃, and the time is 1.4h; the temperature of the heating section 1 is required to be 1205℃, and the time is 1.5h; the temperature of the soaking section is required to be 1200℃, and the time is 1.3h; the steel tapping temperature is 1190℃.

[0151] (7) Rolling process

[0152] Initial rolling temperature is 1000℃, final rolling temperature is 820℃;

[0153] The initial rolling process of continuous casting slab: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 65mm → 2nd pass reduction 70mm → steel turning → 3rd pass reduction 64mm → 4th pass reduction 90mm → steel turning → 5th pass reduction 42mm → 6th pass reduction 40mm → 7th pass reduction 35mm → 8th pass reduction 34mm → steel turning → 9th pass reduction 82mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering the 8-pass continuous rolling unit for rolling.

[0154] Rolling process of the produced material: 8 rolling passes, the 1st pass is 229mm high and 245mm wide; the 2nd pass is 192mm high and 235mm wide; the 3rd pass is 200mm high and 195mm wide; the 4th pass is 169mm high and 212.8mm wide; the 5th pass is 177mm high and 180mm wide; the 6th pass is 141mm high and 192mm wide; the 7th pass is 152mm high and 152mm wide; the 8th pass is 152mm high and 152mm wide; the finished product is produced after 8 passes.

[0155] (8) Insulation process

[0156] Insulation process: Steel insulation, lower insulation pit temperature 580℃, insulation 52h, exit pit temperature 150℃.

[0157] (9) Heat treatment process

[0158] The steel after heat preservation is heat treated, and the heat treatment includes the following steps:

[0159] 1) Quenching: 900℃, holding time 1.0h, oil cooling;

[0160] 2) Tempering: 640℃, keep warm for 2.0h, air cool.

[0161] The macrostructure test results of the steel bars (Φ150 mm) for automotive heat-resistant fasteners prepared in Examples 1-5 are shown in Table 1, the non-metallic inclusion test results are shown in Table 2, and the mechanical properties are shown in Table 3.

[0162] Table 1 Macrostructure test results of steel bars for automotive heat-resistant fasteners prepared in Examples 1-5

[0163]

[0164] Table 2 Non-metallic inclusion detection results of steel bars for automotive heat-resistant fasteners prepared in Examples 1-5

[0165]

[0166] Table 3 Mechanical properties test results of steel bars for automotive heat-resistant fasteners prepared in Examples 1-5

[0167]

[0168] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A steel bar for automotive heat-resistant fasteners, characterized in that: The chemical composition and mass percentage of the steel bar for automobile heat-resistant fasteners are as follows: C: 0.23%-0.27%, Si: 0.20%-0.35%, Mn: 0.42%-0.60%, P: ≤0.015%, S: ≤0.012%, Cr: 1.52%-1.70%, Ni: ≤0.25%, Mo: 0.26%-0.33%, V: 0.16%-0.25%, Cu: ≤0.15%, and the balance is Fe and unavoidable impurities.

2. The production process of steel bars for heat-resistant automotive fasteners according to claim 1, characterized in that: The production process is as follows: ECOARC ecological electric furnace smelting → LF furnace refining → RH refining → continuous casting → annealing → heating furnace heating → rolling → insulation → heat treatment; ECOARC ecological electric furnace smelting process, tapping temperature 1600 ~ 1610 ℃, C 0.08 ~ 0.10%, P ≤ 0.010%, smelting cycle 35 ~ 45min; LF furnace refining process, LF inlet temperature is 1540~1550℃, and molten steel leaves the station when the temperature reaches 1640~1650℃, and LF smelting cycle is 60min~70min; RH refining process, the inlet temperature is 1580-1590℃, the argon pressure is controlled before the vacuum pump is started so that the molten steel is not exposed when the slag surface moves slightly. When the vacuum degree reaches 100-110Pa, the timing starts, and the holding time is 10-15min. Argon is blown statically, the outlet temperature is 1580-1590℃, and the operation time is 40min-50min. In the continuous casting process, the temperature of the ladle at the station is 1565-1575℃, the H in the tundish is controlled to be ≤2ppm, the casting is protected during the whole process, and the mold protection slag uses medium carbon steel protection slag; Annealing process, annealing temperature 640 ~ 650 ℃, annealing time 30 ~ 35h, furnace temperature ≤ 200 ℃; Heating process of heating furnace: the temperature of entering heating furnace is 450℃~560℃, the temperature of soaking section is controlled at 1190℃~1210℃, the time is 1.3~1.5h; the steel tapping temperature is 1185℃~1195℃; Rolling process, initial rolling temperature 1000 ~ 1050 ℃, final rolling temperature 800 ~ 900 ℃; Insulation process, the temperature of the lower insulation pit is 550~590℃, insulation is 50~55h, and the exit temperature is ≤180℃.

3. The production process of steel bars for heat-resistant automotive fasteners according to claim 2, characterized in that: In the ECOARC ecological electric furnace smelting process, slag, pre-deoxidizer and ferroalloy are added when 1 / 4 to 1 / 3 of the steel is tapped. The amount of alloy added per ton of steel: 5.0 to 5.2 kg / t of silicon manganese, 10 to 10.5 kg / t of high carbon ferrochrome, 16 to 16.5 kg / t of low carbon ferrochrome, 1.0 to 1.2 kg / t of aluminum wire segment (10-16 mm); the amount of auxiliary materials added per ton of steel: 40 to 41 kg / t of active lime (10-70 mm), 25 to 26 kg / t of magnesite (10-60 mm), 6 to 6.2 kg / t of ladle ash, 20 to 21 kg / t of small coke pieces, and 18 to 19 kg / t of coking CDQ powder.

4. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: The ECOARC ecological electric furnace smelting process uses raw materials including 38-45t of molten iron, 20-21t of alloy structural steel offcuts, 43-45t of heavy scrap steel, and 10-11t of lump-type scrap steel.

5. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: In the LF furnace refining process, after the LF enters the station, a large current of 35000~36000A is used to heat and melt the slag. When the slag surface fluctuates and the molten steel and the arc are not exposed, active lime is added. After 5~6 minutes, alloy is added according to the target value of chemical composition, and carbon is added to promote rapid melting and homogenization of the alloy and carbon powder. When the temperature of the molten steel reaches 1600~1610℃, 1.5~1.6kg / t of diffusion deoxidizer alumina balls are added for diffusion deoxidation, and the furnace door is closed for 10~13min.

6. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: In the LF furnace refining process, the additional alloys include: ferrosilicon 1.1-1.2kg / t, high carbon ferromanganese 2.1-2.2kg / t, high carbon ferrochrome 3.9-4.0kg / t, ferromolybdenum 0.4-0.5kg / t, ferrovanadium 3.5-3.6kg / t, aluminum wire (Φ10-Φ12mm) 1-1.1m / t; additional auxiliary materials: active lime 4-4.2kg / t, silicon carbide 2.1-2.2kg / t, coke particles 0.75-0.80kg / t.

7. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: In the RH refining process, the argon pressure is controlled at 0.1-0.3 MPa before the vacuum pump is started. The argon pressure is adjusted to 0.3-0.5 MPa during the static argon blowing process. After the static argon blowing is completed, 2-2.1 m / t of silicon-calcium alloy cored wire (Φ14-Φ14.2 mm) and 0.6-0.7 kg / t of covering agent are added.

8. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: In the heating process of the heating furnace, the temperature of the preheating section is controlled at 660℃~700℃, and the time is 1.3~1.5h; the temperature of the heating section 2 is controlled at 850℃~860℃, and the time is 1.3~1.5h; the temperature of the heating section 1 is controlled at 1190℃~1220℃, and the time is 1.3~1.5h.

9. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: Rolling process, continuous casting billet initial rolling process: rolling 9 times, rolling reduction: steel turning → 1st pass reduction 64.9~65.1mm → 2nd pass reduction 69.9~70.1mm → steel turning → 3rd pass reduction 63.9~64.1mm → 4th pass reduction 89.9~90.1mm → steel turning → 5th pass reduction 41.9~42.1mm → 6th pass reduction 39.9~40.1mm → 7th pass reduction 34.9~35.1mm → 8th pass reduction 33.9~34.1mm → steel turning → 9th pass reduction 81.9~82.1mm, passing through 3 850mm rolling mills, 1 735mm rolling mill, and then entering 8 continuous rolling mills for rolling; Rolling process: 8 passes, the first pass is 228.9-229.1mm high and 244.9-245.1mm wide; the second pass is 191.9-192.1mm high and 234.9-235.1mm wide; the third pass is 199.9-200.1mm high and 194.9-195.1mm wide; the fourth pass is 168.9-169.1mm high and 212.7-212.9mm wide mm; the 5th pass is 176.9~177.1mm high and 179.9~180.1mm wide; the 6th pass is 140.9~141.1mm high and 191.9~192.1mm wide; the 7th pass is 151.9~152.1mm high and 151.9~152.1mm wide; the 8th pass is 151.9~152.1mm high and 151.9~152.1mm wide; the finished product is produced after 8 passes.

10. The production process of steel bars for automotive heat-resistant fasteners according to claim 2, characterized in that: The heat treatment process includes the following steps: 1) Quenching: 890-910°C, insulation 0.9-1.2h, oil cooling; 2) Tempering: 630-650℃, keep warm for 1.9-2.2h, air cooling.

Citation Information

Patent Citations

  • Heat resisting type alloy structure steel plate and method for producing same

    CN101724783A

  • High-temperature bolt steel BG25Cr2MoVA and preparation method thereof

    CN108531815A

  • 25Cr2MoVA steel plate for alloy structure and production method thereof

    CN110835712A

  • Production and preparation method of steel bar for ecological electric furnace automobile shaft sleeve

    CN116837291A

  • Preparation method of steel for automobile engine rotor

    CN117758142A

Cited By

  • Production and preparation method of high-temperature-resistant steel bar for automobile axle

    CN119640130A

  • A method for producing a high-temperature-resistant steel bar for automobile axle

    CN119640130B

  • Steel bar for engine crankshaft and production method of steel bar

    CN121874659A

  • A steel bar for engine crankshaft and its manufacturing method

    CN121874659B