A high temperature resistant Hf6Ta2O with hierarchical porous structure 17 Preparation method and application of aerogel

By preparing aerogel with a graded porous structure in Hf6Ta2O17 material, the problem of lack of pore structure of the dense body of the material is solved, high stability and low thermal conductivity are achieved, and its application potential in high temperature environments is enhanced.

CN118307035BActive Publication Date: 2024-11-19YANTAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410426506.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2024-11-19
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

The existing Hf6Ta2O17 dense body lacks pore structure, which limits its application potential in high-temperature environments, making it difficult to achieve precise control of porous structures while ensuring high-temperature resistance.

Method used

The hafnium salt and tantalum salt are hydrolyzed in an organic solvent to form a wet gel. After drying and heat treatment, an Hf6Ta2O17 aerogel with a graded porous structure was prepared. The pore structure and pore size distribution are regulated by controlling the reaction conditions and adding a coagulant.

Benefits of technology

The high stability, low thermal conductivity and high specific surface area of ​​Hf6Ta2O17 aerogel are achieved, which enhances its thermal stability and chemical inertia in high temperature environments, and is suitable for thermal insulation protection in aerospace, nuclear energy and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307035B_ABST
    Figure CN118307035B_ABST
Patent Text Reader

Abstract

The invention discloses a high temperature resistant Hf6Ta2O 17 The preparation method and application of aerogels belong to the technical field of high temperature resistant material preparation. The preparation method comprises the steps of: dissolving hafnium salt and tantalum salt in an organic solvent, adding water to hydrolyze, adding a coagulant and standing to form a wet gel, and drying to obtain Hf6Ta2O 17 Aerogel precursor, Hf6Ta2O 17 The aerogel precursor was heat treated to obtain high temperature resistant Hf6Ta2O with hierarchical porous structure. 17 Aerogel. The Hf6Ta2O 17 Aerogel has a multi-level porous structure, is resistant to high temperatures and heat-insulating, has a complete structure that is not prone to thermal decomposition or phase change, and can resist chemical corrosion and oxidation. It can be widely used in high-temperature working environments such as aerospace, nuclear energy, and chemical industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high temperature resistant material preparation, and specifically relates to a high temperature resistant Hf6Ta2O 17 Preparation method and application of aerogel. Background Art

[0002] With the rapid development of modern science and technology, high temperature resistant materials are increasingly used in aerospace, nuclear energy, electronic devices, chemical industry and other fields. These fields have extremely high requirements for the stability, strength and chemical inertness of materials in high temperature environments. Therefore, the development of new high temperature resistant materials has become one of the important directions of materials science research.

[0003] Hf6Ta2O 17 As a material with excellent high temperature resistance, it has received widespread attention in recent years. The compound has a high melting point, high thermal stability and good chemical inertness, which enables it to maintain structural stability and performance durability in high temperature environments. However, traditional Hf6Ta2O 17 Most of the materials are dense bodies and lack pore structures inside, which to some extent limits their application in certain fields.

[0004] Aerogel, as a material with a unique porous structure, has the advantages of high specific surface area, low density and good thermal insulation performance. 17 Combined with the high temperature resistance of 17 Aerogel.

[0005] In high temperature resistant Hf6Ta2O 17 In the process of preparing aerogels, researchers have tried to construct porous structures through various methods such as sol-gel method and template method. These methods can effectively control the pore size and pore distribution of the material, thereby achieving the regulation of material properties. However, how to achieve precise control of its porous structure while ensuring the high temperature resistance of the material is still a difficulty and hot spot in current research. Summary of the invention

[0006] The purpose of the present invention is to provide a high temperature resistant Hf6Ta2O 17 Preparation method and application of aerogel.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] One of the technical solutions of the present invention is to provide a high temperature resistant Hf6Ta2O with a hierarchical porous structure. 17 The method for preparing aerogel comprises the following steps:

[0009] Dissolve hafnium salt and tantalum salt in an organic solvent, add water to hydrolyze, add a coagulant and let stand to form a wet gel, and then dry to obtain Hf6Ta2O 17 Aerogel precursor, Hf6Ta2O 17 The aerogel precursor was heat treated to obtain high temperature resistant Hf6Ta2O with hierarchical porous structure. 17 Aerogel.

[0010] Preferably, the molar ratio of the hafnium element in the hafnium salt to the tantalum element in the tantalum salt is 3:1; the hafnium salt is hafnium n-butoxide or hafnium chloride; and the tantalum salt is tantalum ethoxide or tantalum chloride.

[0011] Preferably, the organic solvent is ethanol.

[0012] Preferably, the coagulant is propylene oxide.

[0013] More preferably, the standing temperature is 80 to 160° C., and the standing time is 2 to 12 hours.

[0014] Preferably, the drying method is supercritical carbon dioxide drying.

[0015] Preferably, the drying further includes an organic solvent replacement and impurity removal step.

[0016] More preferably, the organic solvent replacement and impurity removal step is to place the wet gel in an organic solvent, replace the organic solvent once every 12 hours, and replace it 4 times in total to remove impurities in the wet gel.

[0017] Preferably, the heat treatment is performed at a temperature of 600 to 1100° C. for a time of 1 to 2 hours.

[0018] The second technical solution of the present invention is to provide a high temperature resistant Hf6Ta2O having a hierarchical porous structure obtained according to the above preparation method. 17 Aerogel.

[0019] Technical solution three of the present invention: providing a high temperature resistant Hf6Ta2O having a hierarchical porous structure 17 Application of aerogel in high temperature resistant materials.

[0020] Hf6Ta2O 17 The technical principle of aerogel mainly involves the crystal structure of the material itself, the stability of chemical bonds and the hierarchical porous structure characteristics of aerogel. 17 The crystal structure of Hf6Ta2O is highly stable. In this structure, hafnium (Hf), tantalum (Ta) and oxygen (O) atoms are connected to each other through strong ionic or covalent bonds to form a stable lattice. This structure makes Hf6Ta2O 17It can also maintain its structural integrity at high temperatures and is not prone to decomposition or phase change. Secondly, the hierarchical porous structure of the aerogel is also a key factor in achieving high temperature resistance. The hierarchical porous structure means that there are pores of different sizes in the aerogel, including macropores, mesopores and micropores. Aerogel is a three-dimensional network structure formed by interconnected nanoscale units, which is filled with gas. This hierarchical porous structure gives the aerogel low thermal conductivity and high specific surface area, which can effectively reduce the heat transfer rate inside the material and improve the thermal stability of the material. In the preparation of high temperature resistant Hf6Ta2O 17 When aerogel is used, Hf6Ta2O 17 The precursor is dispersed in a solvent and formed into a three-dimensional network structure through specific methods (such as sol-gel method, supercritical drying method, etc.). In this process, the pore structure, pore size distribution and porosity of the aerogel can be regulated by controlling the reaction conditions, adding surfactants or template agents, and optimizing its high temperature resistance. In addition, in order to improve the Hf6Ta2O 17 The high temperature resistance of aerogel can also be improved by surface modification or doping with other elements. For example, by introducing a layer of high temperature resistant coating on the surface of aerogel or doping with elements with high thermal stability, its ability to resist high temperature oxidation can be further improved. 17 The technical principle of aerogel mainly relies on its stable crystal structure, the hierarchical porous structure characteristics of aerogel, and the regulation of material properties through preparation methods and surface modification. These characteristics make Hf6Ta2O 17 Aerogel has excellent thermal stability and application potential in high temperature environments.

[0021] The beneficial technical effects of the present invention are as follows:

[0022] Hf6Ta2O prepared by the present invention 17 The aerogel crystal structure is highly stable, which enables the aerogel to maintain structural integrity in high temperature environments and is not prone to thermal decomposition or phase change. The aerogel has a multi-level pore structure, including macropores, mesopores and micropores. This structure provides a large specific surface area and porosity, which helps to improve its thermal, mechanical and transmission properties. In addition, since the aerogel is filled with gas, its thermal conductivity is extremely low, which makes it have excellent thermal insulation properties in high temperature environments. Hf6Ta2O 17 Aerogels have excellent stability to a variety of chemical environments and are resistant to chemical corrosion and oxidation.

[0023] Due to its high temperature resistance and thermal insulation properties, Hf6Ta2O 17 Aerogel can be widely used in high-temperature working environments such as aerospace, nuclear energy, and chemical industry, providing effective thermal insulation protection for equipment in these fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Hf6Ta2O prepared in Example 1 17 X-ray diffraction pattern of aerogel.

[0025] Figure 2 Hf6Ta2O prepared in Example 1 17 Nitrogen adsorption-desorption isotherms of aerogels.

[0026] Figure 3 Hf6Ta2O prepared in Example 1 17 Scanning electron micrograph of aerogel.

[0027] Figure 4 Hf6Ta2O prepared in Example 1 17 Stress-strain curves of aerogels.

[0028] Figure 5 Hf6Ta2O prepared in Example 1 17 Macroscopic image of aerogel.

[0029] Figure 6 Hf6Ta2O prepared in Example 2 17 X-ray diffraction pattern of aerogel.

[0030] Figure 7 Hf6Ta2O prepared in Example 3 17 X-ray diffraction pattern of aerogel.

[0031] Figure 8 Hf6Ta2O prepared in Example 4 17 X-ray diffraction pattern of aerogel.

[0032] Fig. 9 Hf6Ta2O prepared in Example 5 17 X-ray diffraction pattern of aerogel. DETAILED DESCRIPTION

[0033] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0034] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0035] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] Example 1

[0038] Hf6Ta2O 17 Preparation of aerogel:

[0039] (1) Hafnium n-butoxide (3.8 g, 0.00468 mol) and tantalum ethoxide (0.63 g, 0.00156 mol) were first dissolved in 10 mL of ethanol at room temperature, and then 2 mL of deionized water was added thereto. The mixture was stirred in a water bath at 40°C for 1 h.

[0040] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 80° C. for 12 h. After the reaction, a wet gel was formed.

[0041] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0042] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17 Aerogel precursors.

[0043] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 1100 °C for 2 h to obtain Hf6Ta2O 17 Aerogel.

[0044] Figure 1 Hf6Ta2O prepared in Example 1 17 X-ray diffraction diagram of aerogel (the upper line in the figure is the sample curve, and the lower curve is Hf6Ta2O 17 Standard cards).

[0045] from Figure 1 It can be seen that compared with the known crystal structure database, Hf6Ta2O 17 The spectrum of aerogel is similar to that of Hf6Ta2O 17 The data of the standard card correspond to that of the present invention, indicating that Hf6Ta2O 17 Material.

[0046] Figure 2 Hf6Ta2O prepared in Example 1 17 Nitrogen adsorption-desorption isotherms of aerogels.

[0047] according to Figure 2 It can be calculated that Hf6Ta2O 17 The specific surface area of ​​aerogel is about 860m 2 ·g -1 From the nitrogen adsorption-desorption isotherms, it can be seen that in the relative pressure (P / P0) range of 0-0.05, Hf6Ta2O 17 The nitrogen adsorption of the aerogel increased significantly, indicating the presence of a large number of micropores; in the relative pressure (P / P0) range of 0.5-1.0, Hf6Ta2O 17 The aerogel exhibits an obvious hysteresis loop, indicating the presence of a mesoporous structure; in the relative pressure (P / P0) range of 0.8-1.0, Hf6Ta2O 17 The nitrogen adsorption of the aerogel increased dramatically, indicating the presence of many macropores. 17 Aerogels contain both micropores, mesopores and macropores, thus presenting a hierarchical porous structure.

[0048] Figure 3 Hf6Ta2O prepared in Example 1 17 Scanning electron micrograph of aerogel.

[0049] from Figure 3 It can be seen that Hf6Ta2O 17 Aerogel is mainly composed of particles with a porous network structure.

[0050] Figure 4 Hf6Ta2O prepared in Example 1 17 Stress-strain curves of aerogels.

[0051] According to the stress-strain curve, it can be calculated that Hf6Ta2O 17 The compression modulus of the aerogel is 0.6 MPa.

[0052] Figure 5 Hf6Ta2O prepared in Example 1 17 Macroscopic image of aerogel.

[0053] Further determination of Hf6Ta2O prepared in Example 1 17 Thermal conductivity of aerogel. Results: Thermal conductivity at room temperature is 0.023 W·m -1 ·K -1 , the thermal conductivity at 800℃ is 0.045W·m -1 ·K -1 .

[0054] Example 2

[0055] Hf6Ta2O 17 Preparation of aerogel:

[0056] (1) Hafnium n-butoxide (3.8 g, 0.00468 mol) and tantalum ethoxide (0.63 g, 0.00156 mol) were first dissolved in 10 mL of ethanol at room temperature, and then 2 mL of deionized water was added thereto. The mixture was stirred in a water bath at 40°C for 1 h.

[0057] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 120° C. for 12 h. After the reaction, a wet gel was formed.

[0058] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0059] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17 Aerogel precursors.

[0060] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 700 °C for 1 h to obtain Hf6Ta2O 17 Aerogel.

[0061] Figure 6 Hf6Ta2O prepared in Example 2 17 X-ray diffraction diagram of aerogel (the upper line in the figure is the sample curve, and the lower curve is Hf6Ta2O 17 Standard cards).

[0062] from Figure 6 It can be seen that compared with the known crystal structure database, Hf6Ta2O 17 The spectrum of aerogel is similar to that of Hf6Ta2O 17 The data of the standard card correspond to that of the present invention, indicating that Hf6Ta2O 17 Material.

[0063] Example 3

[0064] Hf6Ta2O 17 Preparation of aerogel:

[0065] (1) Hafnium n-butoxide (3.8 g, 0.00468 mol) and tantalum ethoxide (0.63 g, 0.00156 mol) were first dissolved in 10 mL of ethanol at room temperature, and then 2 mL of deionized water was added thereto. The mixture was stirred in a water bath at 40°C for 1 h.

[0066] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 160° C. for 6 h. After the reaction, a wet gel was formed.

[0067] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0068] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17 Aerogel precursors.

[0069] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 800 °C for 1 h to obtain Hf6Ta2O 17 Aerogel.

[0070] Figure 7 Hf6Ta2O prepared in Example 3 17 X-ray diffraction diagram of aerogel (the upper line in the figure is the sample curve, and the lower curve is Hf6Ta2O 17 Standard cards).

[0071] from Figure 7 It can be seen that compared with the known crystal structure database, Hf6Ta2O 17 The spectrum of aerogel is similar to that of Hf6Ta2O 17 The data of the standard card correspond to that of the present invention, indicating that Hf6Ta2O 17 Material.

[0072] Example 4

[0073] Hf6Ta2O 17 Preparation of aerogel:

[0074] (1) Hafnium n-butoxide (3.8 g, 0.00468 mol) and tantalum ethoxide (0.63 g, 0.00156 mol) were first dissolved in 10 mL of ethanol at room temperature, and then 2 mL of deionized water was added thereto. The mixture was stirred in a water bath at 40°C for 1 h.

[0075] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 180° C. for 3 h. After the reaction, a wet gel was formed.

[0076] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0077] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17 Aerogel precursors.

[0078] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 1000 °C for 2 h to obtain Hf6Ta2O 17 Aerogel.

[0079] Figure 8 Hf6Ta2O prepared in Example 4 17 X-ray diffraction diagram of aerogel (the upper line in the figure is the sample curve, and the lower curve is Hf6Ta2O 17 Standard cards).

[0080] from Figure 8 It can be seen that compared with the known crystal structure database, Hf6Ta2O 17 The spectrum of aerogel is similar to that of Hf6Ta2O 17 The data of the standard card correspond to that of the present invention, indicating that Hf6Ta2O 17 Material.

[0081] Example 5

[0082] Hf6Ta2O 17 Preparation of aerogel:

[0083] (1) Hafnium chloride (1.5 g, 0.00468 mol) and tantalum chloride (0.56 g, 0.00156 mol) were dissolved in 10 mL of ethanol at room temperature. 2 mL of deionized water was then added and stirred in a water bath at 40°C for 1 h.

[0084] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 120° C. for 12 h. After the reaction, a wet gel was formed.

[0085] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0086] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17Aerogel precursors.

[0087] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 1000 °C for 1 h to obtain Hf6Ta2O 17 Aerogel.

[0088] Example 6

[0089] Hf6Ta2O 17 Preparation of aerogel:

[0090] (1) Hafnium n-butoxide (1.5 g, 0.00468 mol) and tantalum ethoxide (0.63 g, 0.00156 mol) were first dissolved in 10 mL of ethanol at room temperature, and then 2 mL of deionized water was added thereto. The mixture was stirred in a water bath at 40°C for 1 h.

[0091] (2) 0.5 mL of propylene oxide was slowly added to the above solution, and the stirring was continued at 40° C. for 10 min, then the stirring was stopped and the solution was allowed to react at 140° C. for 12 h. After the reaction, a wet gel was formed.

[0092] (3) The obtained wet gel was replaced with ethanol every 12 hours for 4 times to remove impurities in the wet gel.

[0093] (4) The obtained wet gel material is dried with supercritical carbon dioxide to obtain Hf6Ta2O 17 Aerogel precursors.

[0094] (5)Hf6Ta2O 17 The aerogel precursor was heat treated in a tube furnace at 900 °C for 1 h to obtain Hf6Ta2O 17 Aerogel.

[0095] Fig. 9 Hf6Ta2O prepared in Example 5 17 X-ray diffraction diagram of aerogel (the upper line in the figure is the sample curve, and the lower curve is Hf6Ta2O 17 Standard cards).

[0096] from Fig. 9 It can be seen that compared with the known crystal structure database, Hf6Ta2O 17 The spectrum of aerogel is similar to that of Hf6Ta2O 17 The data of the standard card correspond to that of the present invention, indicating that Hf6Ta2O 17 Material.

[0097] Hf6Ta2O prepared in Example 2-6 17 Aerogels also have micropores, mesopores and macropores, as well as good mechanical properties and thermal conductivity.

[0098] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A high temperature resistant Hf6Ta2O with hierarchical porous structure 17 The method for preparing aerogel is characterized in that: The following steps are involved: Dissolve hafnium salt and tantalum salt in an organic solvent, add water to hydrolyze, add a coagulant and let stand to form a wet gel, and then dry to obtain Hf6Ta2O 17 Aerogel precursor, Hf6Ta2O 17 The aerogel precursor was heat treated to obtain high temperature resistant Hf6Ta2O with hierarchical porous structure. 17 Aerogel; The organic solvent is ethanol; The coagulant is propylene oxide; The drying method is supercritical carbon dioxide drying; The heat treatment temperature is 600-1100° C. and the time is 1-2 hours.

2. The high temperature resistant Hf6Ta2O having a hierarchical porous structure according to claim 1 17 The method for preparing aerogel is characterized in that: The molar ratio of the hafnium element in the hafnium salt to the tantalum element in the tantalum salt is 3:1; the hafnium salt is hafnium n-butoxide or hafnium chloride; and the tantalum salt is tantalum ethoxide or tantalum chloride.

3. The high temperature resistant Hf6Ta2O having a hierarchical porous structure according to claim 1 17 The method for preparing aerogel is characterized in that: The standing temperature is 80-160° C. and the standing time is 2-12 hours.

4. The high temperature resistant Hf6Ta2O having a hierarchical porous structure according to claim 1 17 The method for preparing aerogel is characterized in that: The drying step also includes an organic solvent replacement and impurity removal step.

5. High temperature resistant Hf6Ta2O with hierarchical porous structure obtained by the preparation method according to any one of claims 1 to 4 17 Aerogel.

6. The high temperature resistant Hf6Ta2O with hierarchical porous structure according to claim 5 17 Application of aerogel in high temperature resistant materials.