Method for preparing clay-based cat litter with cat urine pH value detection function
By using clay-based active silicon source and nano-hectorite combined with microwave progressive irradiation technology and tea residue powder, a low-cost, environmentally friendly clay-based cat litter was prepared, which solved the problem of detecting the pH value of cat urine in the existing technology. Complexity and environmental pollution issues, achieving efficient pH value detection and water absorption performance.
Patent Information
- Application Number
- CN202410757421.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-13
AI Technical Summary
In terms of detecting the pH value of cat urine, the existing technology has problems such as complex mass production processes, high costs, and complex preparation ingredients that affect the indication effect. In addition, a large number of chemicals are used in the traditional cat litter preparation process, resulting in environmental pollution.
Using clay-based active silicon source and nanohectorite as the main raw materials, combined with microwave progressive irradiation and solid-phase methods, a clay-based cat litter with pH indicating function was prepared, which reduced the use of chemicals and passed the tea leaves Slag powder serves as an adsorption and odor modification unit, reducing environmental pollution.
It realizes a low-cost, environmentally friendly cat urine pH value detection function, reduces the pollution problem in the traditional cat litter preparation process, improves the water absorption capacity and color development time of cat litter, and avoids environmental pollution.
Smart Images

Figure CN118318739B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cat litter, and in particular to a method for preparing clay-based cat litter with a cat urine pH value detection function. Background Art
[0002] Cat litter is an object used by cat owners to bury feces and urine. It has good water absorption and is generally used together with a cat litter box (or cat toilet). Early cat litters were mainly non-condensing cat litters, mainly for collecting cat feces. In recent years, with the continuous improvement and progress of science and technology and the improvement of living standards, the cat litter industry has also made great progress, and different types of cat litters such as condensed litter, wood litter, crystal litter, bentonite litter, etc. have been born.
[0003] The cat litter made by the prior art is generally made of pulp as raw material, which is beaten into small particles to simulate sand and provide water absorption. In recent years, there are also technical reports using silica gel, corn flour, starch, and plant fiber as adsorption and synthetic raw materials for the preparation of industrial cat litter. In the process of making cat litter, it is usually possible to add chemical products such as antibacterial agents, deodorants, and preservatives to give it certain functionality (such as bactericidal properties, deodorizing properties, preservative properties, dust prevention, etc.), which has led to a series of new methods for preparing cat litter. However, there are few patented technologies for detecting the pH value of cat urine and then monitoring its health. Prior art CN110521613A discloses a cat urine indicator cat litter and a preparation method thereof, which uses deodorant, fiber powder, granules, adhesives, starch, and silica gel as cat litter matrix, and adds pH indicator bromocresol green and phenolphthalein to make it. If the pH value is lower than 5.4, the indicator shows blue-green to yellow, and when the pH value is greater than 8.2, the indicator shows light red to purple. CN116158356A discloses another cat urine indicator cat litter and its preparation method, which is made of bean dregs, corn flour, corn starch, flour, puffed corn flour, calcium carbonate, plant fiber, emulsified balanced oil powder, guar gum, sodium polyacrylate as cat litter matrix, and pH indicator bromothymol blue is added to make it. It can keep color when the pH of urine is 6.0-7.8; it will turn blue when the pH of urine is above 7.6; it will turn yellow when the pH of urine is below 6.0. Recently, Disclosed is a technical method for using purple sweet potato anthocyanins, curcumin and bromothymol blue in combination, and further improving the color development effect of the composition with a specific pH indicator combination, so that the color change interval is more in line with the normal pH range of cat urine, and the color development time is further extended. The above technologies can all achieve the purpose of detection, but there are still practical problems such as complex mass production processes, high costs, and complex preparation ingredients of cat litter that affect the indication effect. Based on the above problems, we further proposed a method for preparing clay-based cat litter with cat urine pH detection function. Summary of the invention
[0004] The purpose of the present invention is to provide a cat litter additive for detecting the pH value of cat urine and a preparation method and application thereof in view of the deficiencies of the existing technical solutions.
[0005] The present invention is achieved through the following technical scheme: a method for preparing a clay-based cat litter with a function of detecting the pH value of cat urine, wherein the cat litter comprises the following raw materials in parts by weight: 50-70% of a clay-based active silicon source, 5-10% of a clay-based nano-lithium laponite, 0.1-10% of tea residue powder, 0.005-0.1% of a pH indicator, 0.1-1% of graphene, and the remainder is ionized water.
[0006] The preparation method is as follows:
[0007] S1. Mixing the clay-based nano-hectorite with water, stirring with a stirrer, the stirring speed is 1000-7000 rpm, the stirring temperature is 25-40°C, the stirring time is 0.5-3 h, and the obtained raw material is recorded as material 1;
[0008] S2. Mix the clay-based active silicon source, pH indicator, graphene, and water with a stirrer. After mixing evenly, transfer the resulting mixed solution to a microwave digestion tank. Place the microwave digestion tank in a microwave digestion instrument for reaction. The reaction conditions are: reaction temperature 100-160°C, irradiation frequency: 100w irradiation 10s, 150w irradiation 10s, 200w irradiation 10s, 250w irradiation 10s, 350w irradiation 10s, stop 10s, irradiation cycle 10-30. After the reaction is completed, take it out and the resulting product is recorded as material 2;
[0009] S3. Mix material 1, material 2 and tea residue powder, stir evenly, take out and extrude granules, and after granulation, place them in a constant temperature oven for drying. The drying temperature is 85-90℃, the drying time is 6-12h; the granulator power is 100-150 W, the granulation temperature is 60-70℃, and the cat litter particle size obtained by granulation is 1-3 mm.
[0010] The method for preparing the clay-based active silicon source is as follows:
[0011] S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0012] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g:2.5ml-5ml;
[0013] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 110 - 200 ℃, and the irradiation cycle is 30;
[0014] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0015] Furthermore, the natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite;
[0016] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L;
[0017] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0018] Furthermore, the irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s.
[0019] The method for preparing the clay-based nano-hectorite is as follows:
[0020] A. Mix the lithium source, magnesium source, and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir thoroughly, transfer to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 9-12;
[0021] B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The irradiation conditions are: irradiation temperature is 110-180°C and irradiation cycle is 10-30;
[0022] C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0023] Furthermore, in step A, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two.
[0024] Furthermore, the irradiation cycle mentioned in step B is specifically each cycle of 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0025] The graphene has a flake lateral distance of 1-2 μm and a carbon-oxygen ratio of 4-7.
[0026] The pH indicator is any one of bromocresol green, bromothymol blue, turmeric and bromothymol blue.
[0027] The tea residue powder is obtained by drying and crushing the tea waste produced after drinking jasmine tea, Tieguanyin tea, white tea and Longjing tea. The specific drying conditions are 50-70°C and the drying time is 12-24 hours. The dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain tea residue powder;
[0028] Furthermore, in the process of preparing the clay-based cat litter, the tea residues selected are a mixture of one or more of jasmine tea, Tieguanyin tea, white tea, and Longjing tea residues.
[0029] Beneficial effects of the present invention: First, in terms of synthetic raw materials, this method is completely different from the main raw materials for preparing cat litter at present. The silicon source we use is the silicon source produced by acid depolymerization of natural clay as the synthetic raw material (i.e., clay-based active silicon source), which to a certain extent alleviates the problem of upper-end pollution of synthetic raw materials caused by the use of silicon-containing chemicals (such as silica gel) in the traditional cat litter preparation process, and reduces the synthesis cost of cat litter. In addition, for the process of obtaining clay-based active silicon sources, we have originally proposed and adopted a superimposed composite process of a solid-phase method and a microwave progressive irradiation method, that is, firstly, natural clay is separated from acid solution in a microwave digestion tank, and microwave irradiation is used to heat and evaporate the acid solution to produce acid vapor, which then reacts with natural clay. The advantage of this is that, on the one hand, low-concentration acid solution can play the effect of high-concentration acid solution, effectively improve the use efficiency of acid solution, and at the same time, it can also be recycled multiple times by appropriately adding a small amount of acid solution. In addition, a large amount of high-value elements, such as aluminum and potassium, can be present in the acid solution, which can be effectively enriched through the above process to facilitate the high-value-added utilization of clay minerals.
[0030] Secondly, under the environment of this microwave progressive irradiation, under the influence of the solid-phase system, the natural clay powder is directly irradiated by microwaves. Since different chemical bonds receive microwaves differently, they can be directly activated, and the chemical bond activation and broken parts will be consistent. This is not only the reason why natural clay can be depolymerized without a high-temperature activation step in the technology of the present invention. At the same time, this broken chemical bond can better combine with the pH indicator firmly and evenly through chemical interactions. Through the action of microwaves, the loading method of the nano pH indicator can be further identified (under this condition, the pH indicator can only be combined chemically, and physical adsorption is eliminated), avoiding excessive use of the pH indicator.
[0031] Again, in the present invention, nano lithium soapstone (clay-based active silicon source as the synthetic raw material of nano lithium soapstone) and tea residue powder are used as cat litter adsorption units and odor modification units, which not only eliminates the addition of chemicals (chemical synthetic flavors) again, but also further makes the process of synthesizing cat litter greener. It is noted again that because the clay-based active silicon source we obtained has ultra-high activity, if the traditional microwave synthesis method is directly used, due to the uncontrollable heat supply, the crystal nucleus will grow rapidly through the Oswald reaction after generation, and the lithium soapstone obtained will show the characteristics of chaotic crystal size distribution. However, when using microwave progressive irradiation, since the chemical bonds broken by the silicon raw material are consistent, and the heat supply method is regularized, it is beneficial to obtain nano lithium soapstone with uniform morphology, which is extremely beneficial to improving the water absorption capacity of cat litter.
[0032] Finally, since only pollution-free natural components are used in the production process of cat litter, no additional chemical components are added, and the pH indicator content is also very low (0.005-0.1%), after the cat litter is used, it can be discharged into the natural environment as solid fertilizer, avoiding the environmental pollution caused by the discharge of discarded cat litter. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0034] Figure 1 This is the XRD diagram of the clay-based active silicon source in Example 1.
[0035] Figure 2 This is the XRD diagram of clay-based nano-lithium laponite in Example 1.
[0036] Figure 3 This is the SEM image of the clay-based nano-lithium laponite in Example 1.
[0037] Figure 4 This is an actual picture of the S1 material produced by mixing the clay-based nano-hectorite and water described in Example 1. DETAILED DESCRIPTION
[0038] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification:
[0039] Embodiment 1:
[0040] A method for preparing a clay-based cat litter with a function of detecting the pH value of cat urine. The cat litter comprises the following raw materials in parts by weight: 70% of a clay-based active silicon source, 10% of a clay-based nano-lithium laponite, 10% of tea residue powder, 0.1% of a pH indicator, 1% of graphene, and the remainder being ionized water.
[0041] The preparation method is as follows:
[0042] S1. The clay-based nano-hectorite was mixed with water and stirred with a stirrer at a stirring speed of 7000 rpm, a stirring temperature of 25°C, and a stirring time of 0.5 h. The obtained raw material was recorded as material 1;
[0043] S2. Mix the clay-based active silicon source, pH indicator, graphene and water with a stirrer. After mixing evenly, transfer the resulting mixed solution to a microwave digestion tank. Place the microwave digestion tank in a microwave digestion instrument to react. The reaction conditions are: reaction temperature 160°C, 10 irradiation cycles. After the reaction is completed, take it out and the resulting product is recorded as material 2.
[0044] The irradiation cycle mentioned in step S2 is specifically that each cycle is 100w irradiation for 10s, 150w irradiation for 10s, 200w irradiation for 10s, 250w irradiation for 10s, 350w irradiation for 10s, and stop for 10s;
[0045] S3. Mix material 1, material 2, and tea residue powder, stir evenly, take out and extrude granules, and after granulation, place them in a constant temperature oven for drying. The drying temperature is 90℃, and the drying time is 6 h; the granulator power is 150W, the granulation temperature is 60℃, and the cat litter particle size obtained by granulation is 1 mm.
[0046] Furthermore, the pH indicator is bromocresol green.
[0047] The method for preparing the clay-based active silicon source is as follows:
[0048] S1, selecting natural clay ore, flotation separation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder;
[0049] S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g:2.5ml;
[0050] S3, the microwave digestion tank installed in step S2 is loaded into a microwave digestion instrument, and irradiated according to specific irradiation conditions, specifically, the irradiation temperature is 110 ° C, and the irradiation cycle is 30;
[0051] S4, take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is the clay-based active silicon source;
[0052] Furthermore, the natural clay in step S1 is kaolin;
[0053] Furthermore, the acid solution used in step S2 is hydrochloric acid, and its concentration is 4 mol / L;
[0054] Furthermore, in step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium.
[0055] Furthermore, the irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s.
[0056] The method for preparing the clay-based nano-hectorite is as follows:
[0057] A. Mix the lithium source, magnesium source, and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir thoroughly, transfer to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 12;
[0058] B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The irradiation conditions are: irradiation temperature is 110°C and irradiation cycle is 30;
[0059] C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-lithium laponite.
[0060] Furthermore, in step A, the lithium source is lithium carbonate; and the magnesium source is magnesium chloride.
[0061] Furthermore, the irradiation cycle mentioned in step B is specifically each cycle of 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
[0062] The graphene has a flake lateral distance of 1 μm and a carbon-oxygen ratio of 7.
[0063] The tea residue powder is obtained by drying and crushing the tea waste produced by drinking jasmine tea. The specific drying conditions are 70°C and the drying time is 24 hours. The dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain tea residue powder;
[0064] from Figure 1 It can be seen that the clay-based active silicon source product presents an amorphous structure, indicating that its inherent crystal structure has been completely depolymerized into active species suitable for synthesizing hectorite.
[0065] Figure 2 This is the XRD diagram of the product nano-hectorite in Example 1. Based on its diffraction peak, it can be determined that the synthesized product is nano-hectorite, which further proves that it is synthesized from a clay-based active silicon source.
[0066] Figure 3 This is a SEM image of the clay-based nano-lithium laponite recorded in Example 1. As can be seen from the figure, the clay-based nano-lithium laponite obtained under the experimental environment of Example 1 presents a relatively uniform flaky morphology at the nanoscale.
[0067] Figure 4 This is an actual picture of the S1 material produced by mixing the clay-based nano-hectorite and water recorded in Example 1. The picture shows 100 ml of water mixed with 0.3 g of clay-based nano-hectorite, which can prove that it has excellent water absorption and gelation ability.
[0068] The rest of Example 2 is the same as Example 1, except that the cat litter is prepared by comprising the following raw materials in parts by weight: 50% clay-based active silicon source, 5% clay-based nano-lithium laponite, 0.4% tea residue powder, 0.01% pH indicator, 0.5% graphene, and the balance is ionized water.
[0069] The rest of Example 3 is the same as Example 1, except that in step S1, the stirring speed is 1500 rpm, the stirring temperature is 30°C, and the stirring time is 1 h; in step S2, the reaction temperature is 100°C, the irradiation cycle is 30, and the hydrochloric acid concentration is 2 mol / L; the pH indicator used is bromothymol blue.
[0070] The rest of Example 4 is the same as Example 1, except that, in step S3, the irradiation temperature is 200°C, and the irradiation cycle is 30; the drying temperature is 85°C, and the drying time is 12 h; the cat litter particle size is 2 mm; the pH indicator is turmeric; the tea residue selected is Tieguanyin tea residue, and further, the drying condition is 50°C, and the drying time is 12 h.
[0071] The rest of Example 5 is the same as Example 1, except that, in step S3, the granulator power is 100 W, the granulation temperature is 70° C., the cat litter particle size is 2 mm, the pH indicator is bromothymol blue, and the tea residues used are Longjing tea residues.
[0072] The rest of Example 6 is the same as Example 1, except that in step A, ammonia water is added dropwise to maintain the pH of the reaction system at 9; in step B, the irradiation temperature is 180°C, and the irradiation cycle is 12; the natural clay selected is montmorillonite.
[0073] The rest of Example 7 is the same as Example 1, except that the natural clay selected is rectorite; the graphene used in step S2 has a flake lateral distance of 2 μm and a carbon-oxygen ratio of 4.
[0074] The rest of Example 8 is the same as Example 1, except that the lithium source is lithium fluoride and the magnesium source is magnesium hydroxide.
[0075] Experimental data:
[0076] serial number Water absorption (%) Color development time(s) Moisture determination (%) Example 1 738 4 S 0.7 Example 2 729 7 S 0.8 Example 3 743 5 S 0.5 Example 4 736 6 S 0.7 Example 5 728 4 S 0.6 Example 6 732 4 S 0.7 Example 7 734 4 S 0.6 Example 8 734 4 S 0.7
[0077] Water absorption test:
[0078] 1. Place the standard sieve in a stainless steel pan filled with water, making the water level about 5 mm above the sieve, and soak for 10 seconds.
[0079] 2. Take out the wet standard sieve from the water container, place it at a 30° angle for 5 minutes, and then weigh the wet standard sieve.
[0080] 3. Accurately weigh 10.0 g of the cat litter sample obtained under the conditions of each embodiment that has been dried to constant weight at 105°C ± 5°C, place it in a wet standard sieve, and spread the sample evenly on about 1 / 2 of the sieve surface.
[0081] 4. Slowly immerse the standard sieve and the sample into the water container. During the water absorption process, make sure the water surface always submerges the cat litter sample.
[0082] 5. After absorbing water for 5 minutes, slowly take out the standard sieve containing the wet sample from the water container, place it at a 30° angle for 10 minutes, and then weigh it on a balance.
[0083] The water absorption rate X of the sample is expressed as mass fraction (%) and is calculated according to the formula X=(BAC) / C*100.
[0084] Where: A is the mass of the empty wet sieve, in grams (g); B is the mass of the sample after wet sieve and water absorption, in grams (g); C is the mass of the sample, in grams (g). The arithmetic mean of the results of three parallel measurements is taken as the measurement result.
[0085] Color development time experiment
[0086] The cat litter prepared under the conditions of each embodiment was spread in a basin about 5 cm, and a certain amount of acid-base standard solution with different pH was sucked with a syringe (in the standard solution: the acid solution is hydrochloric acid solution, and the alkaline solution is sodium hydroxide solution). To simulate the process of cat urination, a peristaltic pump was used to pump it into the tested cat litter at a height of about 10 cm (the syringe was installed on the peristaltic pump). A stopwatch was used to record the time required for the test solution to contact the cat litter and develop color. Each group of experiments was performed 5 times, and the average time was taken.
[0087] Moisture determination:
[0088] Weigh 10g of each cat litter prepared under the conditions of each example, place it in a constant temperature oven at 105±2℃, and dry it under atmospheric pressure until constant weight. The lost weight is water. The ratio of the mass of water contained in the sample to the mass of the sample represents the water content in the sample.
[0089] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a clay-based cat litter with a cat urine pH value detection function, characterized in that: The cat litter is prepared by comprising the following raw materials in parts by weight: 50-70% clay-based active silicon source, 5-10% clay-based nano-hectorite, 0.1-10% tea residue powder, 0.005-0.1% pH indicator, 0.1-1% graphene, and the balance is ionized water; The preparation method is as follows: S1. Mixing the clay-based nano-hectorite with water, stirring with a stirrer, the stirring speed is 1000-7000 rpm, the stirring temperature is 25-40°C, the stirring time is 0.5-3 h, and the obtained raw material is recorded as material 1; S2. The clay-based active silicon source, pH indicator, graphene and water are mixed with a stirrer. After being mixed evenly, the obtained mixed solution is transferred to a microwave digestion tank, and the microwave digestion tank is placed in a microwave digestion instrument for reaction. The obtained product is recorded as material 2. The reaction conditions are: reaction temperature 100-160°C, irradiation cycle 10-30; The irradiation cycle mentioned in step S2 is specifically that each cycle is 100w irradiation for 10s, 150w irradiation for 10s, 200w irradiation for 10s, 250w irradiation for 10s, 350w irradiation for 10s, and stop for 10s; S3. Mix material 1 and material 2, as well as tea residue powder, stir evenly, take out and perform extrusion granulation. After granulation, place it in a constant temperature oven and dry it at a temperature of 85-90 ° C for 6-12 h. The granulator power is 100-150 W, the granulation temperature is 60-70 ° C, and the cat litter particle size obtained by granulation is 1-3 mm. The method for preparing the clay-based active silicon source is as follows: S1, selecting natural clay ore, flotation and impurity removal, grinding into powder, and then sieving through a 100-mesh sieve to obtain natural clay powder; S2, natural clay powder and acid solution are loaded into a microwave digestion tank according to a certain solid-liquid ratio, and the ratio range is natural clay (weight): acid solution (volume) = 1g:2.5ml-5ml; S3, loading the microwave digestion vessel prepared in step S2 into a microwave digestion instrument, and irradiating the solution according to specific irradiation conditions, specifically, an irradiation temperature of 110-200° C. and 30 irradiation cycles; S4, taking out the microwave digestion tank after microwave irradiation, filtering the solid product until it is neutral, and placing it in a constant temperature oven at 90° C. to dry for 12 hours. The obtained solid powder is the clay-based active silicon source; The natural clay in step S1 is a mixture of one or more of kaolin, montmorillonite and rectorite; The acid solution used in step S2 is hydrochloric acid, and its concentration is 2-4 mol / L; In step S2, the natural clay and the acid solution are isolated from each other, that is, during the microwave irradiation process, only the acid solution is heated to form acidic steam as the reaction medium; The irradiation cycle mentioned in step S3 is specifically that each cycle is 200w irradiation for 10s, 230w irradiation for 10s, 270w irradiation for 10s, 330w irradiation for 10s, 350w irradiation for 10s, and stop for 10s; The method for preparing the clay-based nano-hectorite is as follows: A. Mix the lithium source, magnesium source and clay-based active silicon source in a molar ratio of 1:3:1.7 and stir them thoroughly, transfer them to a microwave digestion tank, and add ammonia water dropwise to maintain the pH of the reaction system at 9-12; B. Load the prepared microwave digestion tank into the microwave digestion instrument for irradiation reaction. The irradiation conditions are: irradiation temperature is 110-180℃, and the irradiation cycle is 10-30; C. Take out the microwave digestion tank after microwave irradiation, filter the solid product until it is neutral, and place it in a constant temperature oven at 90°C to dry for 12 hours. The obtained solid powder is nano-hectorite; In step A, the lithium source is one of lithium fluoride and lithium carbonate or a mixture of the two; the magnesium source is one of magnesium chloride and magnesium hydroxide or a mixture of the two; The irradiation cycle mentioned in step B is specifically that each cycle is 160W irradiation for 20s, 270W irradiation for 10s, 330W irradiation for 10s, 350W irradiation for 10s, and stop for 10s.
2. According to the method for preparing a clay-based cat litter with a cat urine pH value detection function as claimed in claim 1, the graphene has a flaky lateral distance of 1-2 um and a carbon-oxygen ratio of 4-7.
3. According to the method for preparing a clay-based cat litter with a cat urine pH value detection function as claimed in claim 1, the pH indicator is any one of bromocresol green, bromothymol blue, turmeric, and bromothymol blue.
4. According to the method for preparing a clay-based cat litter with a cat urine pH value detection function as described in claim 1, the tea residue powder is obtained by drying and crushing tea waste produced after drinking jasmine tea, Tieguanyin tea, and Longjing tea, and the specific drying conditions are 50-70° C. and the drying time is 12-24 hours. The dried solid tea residue is crushed and sieved through an 80-mesh sieve to obtain the tea residue powder; In the process of preparing clay-based cat litter, the tea residues selected are a mixture of one or more of jasmine tea, Tieguanyin tea and Longjing tea residues.
Citation Information
Patent Citations
Cat litter and preparing method thereof
CN110521613A
Cat urine PH indicating cat litter and preparation method thereof
CN116158356A
Cat urine pH indicating material, pH indicating silica gel cat sand and preparation method thereof
CN101672799A
Mineral adsorption type cat litter and preparation method thereof
CN104396765A
Method for treating illite to synthesize zeolite molecular sieves by microwave heating solid-like-phase acid steam conversion process