A method for preparing a dual-monomer polymerized polyamide nanofiltration membrane
By homopolymerizing on the support to form a porous PAMPS layer and polymerizing with polyamines and polychlorinated acid chlorides, the existing polyamide nanofiltration membrane has been solved, and the water quality requirements, poor acid and alkali resistance and low water flux are achieved. Improved flux and stability while reducing production costs.
Patent Information
- Application Number
- CN202410675702.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-29
AI Technical Summary
The existing polyamide nanofiltration membranes have strict water quality requirements, poor acid and alkali resistance, low water flux and high production costs. In particular, AMPS is too dense in photoinduced polymerization and affects interface polymerization, which increases the preparation cost.
By homopolymerizing on the support, forming a porous PAMPS polymer layer, and coating polyamine and polyacid chloride, adjusting the polyamine concentration to polymerize PAMPS and acid chloride interfacially, avoiding AMPS homopolymerization affecting the interface polymerization, and forming a high-throughput Polyamide nanofiltration membrane.
It is possible to form a large-flux polyamide nanofiltration membrane on the basis of ensuring retention, which improves the stability and acid and alkali resistance of the membrane, and reduces production costs.
Smart Images

Figure CN118320651B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a polyamide nanofiltration membrane, in particular to a method for preparing a polyamide nanofiltration membrane by AMPS-assisted dual-monomer polymerization. Background Art
[0002] The origin of nanofiltration technology can be traced back to the development of reverse osmosis technology. The operating pressure of nanofiltration is between 0.5-1.5MPa. This technology is also called "loose reverse osmosis" or "low-pressure reverse osmosis". Polyamide nanofiltration membrane is a common type of nanofiltration membrane and is widely used in the field of liquid separation and purification. Its precise pore structure and unique surface chemical properties make it show great application potential in many industrial fields.
[0003] Existing polyamide nanofiltration membranes are often formed by interfacial polymerization of polyamines and polyacyl chlorides. In order to improve hydrophilicity, the prior art discloses the use of polyamines with sulfonic acid groups alone or mixed with other polyamines as water phase monomers, but the polyamide nanofiltration membranes prepared by the above method in the prior art have strict requirements on water quality and cannot be acid, alkali and aluminum resistant. 2-Acrylamide-2-methylpropane sulfonic acid is a multifunctional water-soluble anionic surfactant monomer with a stable structure. It can be used as a water phase monomer to achieve acid, alkali and chlorine resistance. Among them, CN116585894A discloses that AMPS is mixed with diamine monomers as a monomer cross-linking agent, and a polyamide nanofiltration membrane with high cross-linking density is prepared by photo-induced polymerization assisted interfacial polymerization. However, in the prior art, AMPS only plays the role of a cross-linking agent, and because photo-induced polymerization and interfacial polymerization affect each other, the prepared membrane is too dense and the water flux is not high. In addition, photo-induced polymerization requires a more stringent operating environment, which increases the production cost of the membrane.
[0004] In addition, when preparing polyamide nanofiltration membranes, the surface properties of the support will also affect the performance of the final membrane. For this reason, the existing technology often uses an intermediate layer to improve the flatness of the support surface, but the additional intermediate layer will also increase the cost of the membrane. Therefore, how to design AMPS-assisted preparation of polyamide nanofiltration membranes is an urgent problem to be solved. Summary of the invention
[0005] The present invention forms a porous PAMPS polymer layer by homopolymerizing AMPS and porous particles on a support, and then coats polyamine and polyacyl chloride on the porous PAMPS polymer layer, and adjusts the concentration of the polyamine so that the PAMPS and the polyamine are polymerized with the acyl chloride interface to form a polyamide nanofiltration membrane.
[0006] The present invention provides a method for preparing a dual-monomer polymerized polyamide nanofiltration membrane, comprising the following steps:
[0007] (1) pretreating the support to remove impurities;
[0008] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid in a solvent, adding an appropriate amount of an initiator, porous particles and a porogen, and stirring to form a coating liquid;
[0009] (3) uniformly coating the coating liquid on the support, and placing it at a specific temperature for homopolymerization. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0010] (4) coating the support with an aqueous solution containing a diamine monomer, and immersing the support in an organic solution containing a polyacyl chloride after standing for 1-5 minutes to cause an interfacial polymerization reaction;
[0011] (5) Drying the membrane obtained after the reaction to obtain a polyamide nanofiltration membrane.
[0012] Preferably, the pretreatment in step (1) includes soaking in deionized water, ultrasound, and drying steps.
[0013] Preferably, the solvent in step (2) is dimethylformamide, methanol, ethanol or water, and the concentration of 2-acrylamide-2-methylpropanesulfonic acid in the coating liquid is 10-30 wt %.
[0014] Preferably, the initiator in step (2) is one of benzoyl peroxide, azobisisobutyronitrile and diisopropylbenzene hydroperoxide, and the concentration is 0.1wt%-2wt%.
[0015] Preferably, the porous particles in step (2) are microporous zeolites with a particle size of 50-100 nm, a silicon-aluminum ratio of 5-20, and a concentration in the coating liquid of 2-8 wt %.
[0016] Preferably, the porogen in step (2) is one of polyvinyl pyrrolidone and polyethylene glycol, and the concentration in the coating solution is 2-6 wt %.
[0017] Preferably, in step (3), the specific temperature is 50-100° C. and the reaction time is 5-48 h.
[0018] Preferably, the diamine monomer in step (4) is m-phenylenediamine, and the concentration is 0.05-0.5 wt %.
[0019] Preferably, in step (4), the polyacyl chloride is trimesoyl chloride, the concentration is 0.5-2wt%, and the immersion time is 60-120s.
[0020] Preferably, the drying in step (5) is performed at room temperature - 80°C.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] Firstly, the present invention homopolymerizes AMPS and porous particles on a support to form a porous PAMPS polymer layer, and then coats the layer with polyamine and polyacyl chloride, and adjusts the concentration of the polyamine so that both PAMPS and the polyamine are polymerized with the acyl chloride to form a polyamide nanofiltration membrane, thereby avoiding the homopolymerization process of AMPS affecting the interfacial polymerization, thereby forming a polyamide nanofiltration membrane with a large flux while ensuring the rejection rate, and the stability of the polyamide nanofiltration membrane can be improved by the intervention of AMPS.
[0023] Secondly, the present invention forms a porous polymer by coating AMPS on a support body for prepolymerization, thereby avoiding the influence of the support body on the interface polymerization.
[0024] In addition, the porous particle-doped polymer layer formed by the present invention will adsorb the polyamine coated nearby, causing more PAMPS to leak out, and cooperate with the low concentration of polyamine, so that more PAMPS will polymerize with the acyl chloride, thereby increasing the PAMPS content in the polyamide layer, thereby improving the stability of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Attached Figure 1 This is a surface SEM image of the polyamide nanofiltration membrane prepared in Example 1. DETAILED DESCRIPTION
[0026] Example 1
[0027] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0028] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0029] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide, 4 wt% ZSM-5 molecular sieve with a silicon-aluminum ratio of 12 and an average particle size of 78 nm, and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0030] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0031] (4) coating the support with an aqueous solution containing 0.1 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0032] (5) The membrane obtained after the reaction was dried at 60°C to obtain a polyamide nanofiltration membrane (the SEM characterization of the membrane surface is as follows: Figure 1 as shown).
[0033] Example 2
[0034] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0035] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0036] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide, 4 wt% mordenite with a silicon-aluminum ratio of 17 and an average particle size of 98 nm, and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0037] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0038] (4) coating the support with an aqueous solution containing 0.1 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0039] (5) The membrane obtained after the reaction is dried at 60°C to obtain a polyamide nanofiltration membrane.
[0040] Example 3
[0041] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0042] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0043] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0044] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0045] (4) coating the support with an aqueous solution containing 0.1 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0046] (5) The membrane obtained after the reaction is dried at 60°C to obtain a polyamide nanofiltration membrane.
[0047] Example 4
[0048] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0049] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0050] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide, 4 wt% NaA molecular sieve with a silicon-aluminum ratio of 1 and an average particle size of 81 nm, and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0051] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0052] (4) coating the support with an aqueous solution containing 0.1 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0053] (5) The membrane obtained after the reaction is dried at 60°C to obtain a polyamide nanofiltration membrane.
[0054] Example 5
[0055] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0056] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0057] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide, 4 wt% Silicalite-1 molecular sieve having an average particle size of 65 nm and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0058] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0059] (4) coating the support with an aqueous solution containing 0.1 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0060] (5) The membrane obtained after the reaction is dried at 60°C to obtain a polyamide nanofiltration membrane.
[0061] Example 6
[0062] The method for preparing a polyamide nanofiltration membrane prepared by dual-monomer polymerization according to an embodiment of the present invention comprises the following steps:
[0063] (1) A polyethersulfone microfiltration membrane is used as a support, and the support is immersed in deionized water, subjected to ultrasound, and dried to remove impurities;
[0064] (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid (25 wt%) in dimethylformamide, adding 0.5 wt% benzoyl peroxide, 4 wt% ZSM-5 molecular sieve with a silicon-aluminum ratio of 12 and an average particle size of 78 nm, and 4 wt% polyvinyl pyrrolidone, and stirring to form a coating liquid;
[0065] (3) The coating liquid is evenly coated on the support, and the support is placed at 80°C for homopolymerization for 24 hours. After the polymerization is completed, the support is taken out, cooled to room temperature, immersed in deionized water and dried;
[0066] (4) coating the support with an aqueous solution containing 2 wt % of m-phenylenediamine, allowing the support to stand for 2 min, and then immersing the support in an organic solution containing 0.8 wt % of trimesoyl chloride to cause an interfacial polymerization reaction;
[0067] (5) The membrane obtained after the reaction is dried at 60°C to obtain a polyamide nanofiltration membrane.
[0068] The polyamide nanofiltration membrane of the above embodiment was tested for the permeability of magnesium sulfate and sodium chloride. The results are shown in Table 1:
[0069] Table 1
[0070]
[0071] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a dual-monomer polymerized polyamide nanofiltration membrane, characterized in that The method comprises the following steps: (1) pre-treating the support to remove impurities; (2) dissolving 2-acrylamide-2-methylpropanesulfonic acid in a solvent, adding an appropriate amount of an initiator, porous particles and a porogen, and stirring to form a coating liquid; (3) uniformly coating the coating liquid on the support, placing it at a specific temperature for homopolymerization, and after the polymerization is completed, taking out the support, cooling it to room temperature, and soaking it in deionized water and drying it; (4) coating the support with an aqueous solution containing a diamine monomer, and after standing for 1-5 minutes, immersing it in an organic solution containing a polyacyl chloride to cause an interfacial polymerization reaction; (5) drying the membrane obtained after the reaction to obtain a polyamide nanofiltration membrane; the porous particles in step (2) are microporous zeolites with a particle size of 50-100 nm, a silicon-aluminum ratio of 5-20, and a concentration of 2-8 wt % in the coating liquid; the solvent in step (2) is dimethylformamide, methanol, ethanol or water, and the concentration of 2-acrylamide-2-methylpropanesulfonic acid in the coating liquid is 10-30 wt %; the specific temperature in step (3) is 50-100 ° C, and the reaction time is 5-48 h.
2. The preparation method according to claim 1, characterized in that The pretreatment in step (1) includes soaking in deionized water, ultrasound, and drying steps.
3. The preparation method according to claim 1, characterized in that In step (2), the initiator is one of benzoyl peroxide, azobisisobutyronitrile and diisopropylbenzene hydroperoxide, and the concentration in the coating liquid is 0.1wt-2wt%.
4. The preparation method according to claim 1, characterized in that In step (2), the porogen is one of polyvinyl pyrrolidone and polyethylene glycol, and the concentration in the coating solution is 2-6 wt %.
5. The preparation method according to claim 1, characterized in that In step (4), the diamine monomer is m-phenylenediamine, and its concentration in the aqueous solution is 0.05-0.5 wt %.
6. The preparation method according to claim 1, characterized in that In step (4), the polyacid chloride is trimesoyl chloride, the concentration of which in the organic phase solution is 0.5-2wt%, and the immersion time is 60-120s.
7. The preparation method according to claim 1, characterized in that The drying in step (5) is performed at room temperature - 80°C.